General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.82 g/cm³ Show Material materials with Densidad of 2.82 g/cm³ | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Dureza Brinell | 135.0 [-] Show Material materials with Dureza Brinell of 135.0 [-] | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | ||
20.0 °C | 135.0 [-] Show Material materials with Dureza Brinell of 135.0 [-] | T7451 | WL 3.4394 | Plate | ||
Elongación | 8.0 % Show Material materials with Elongación of 8.0 % | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | A50 | |
9.0 % Show Material materials with Elongación of 9.0 % | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | A50 | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T7451 | WL 3.4394 | Plate | ||
Módulo de cizallamiento | 27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | ||
Plane-Strain Fracture Toughnes | 20.0 °C | 24.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | |
20.0 °C | 24.0 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 27.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 27.6 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 26.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 26.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 27.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 27.6 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 26.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 26.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 27.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 27.6 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 34.1 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.1 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 34.1 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.1 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 34.1 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.1 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 35.7 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 35.7 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 35.7 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 35.7 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 39.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 39.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
Resistencia a la tracción | 455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | ||
465.0 MPa Show Material materials with Resistencia a la tracción of 465.0 MPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | |||
480.0 MPa Show Material materials with Resistencia a la tracción of 480.0 MPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | |||
490.0 MPa Show Material materials with Resistencia a la tracción of 490.0 MPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | |||
20.0 °C | 455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 465.0 MPa Show Material materials with Resistencia a la tracción of 465.0 MPa | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 480.0 MPa Show Material materials with Resistencia a la tracción of 480.0 MPa | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 490.0 MPa Show Material materials with Resistencia a la tracción of 490.0 MPa | T7451 | WL 3.4394 | Plate |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 795.0 - 1050.0 J/(kg·K) Show Material materials with Calor específico of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium |
Coeficiente de dilatación térmica | 2.1e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 - 2.4e-05 1/K | Typical for Wrought 7000 Series Aluminium |
Conductividad térmica | 121.0 - 170.0 W/(m·K) Show Material materials with Conductividad térmica of 121.0 - 170.0 W/(m·K) | Typical for Wrought 7000 Series Aluminium |
Temperatura de fusión | 465.0 - 655.0 °C Show Material materials with Temperatura de fusión of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 25000000.0 S/m | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire |
Resistividad eléctrica | 4e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 4.35e-08 Ω·m | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Circonio | 0.1 - 0.16 % Show Material materials with Circonio of 0.1 - 0.16 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Cobre | 1.5 - 2.0 % Show Material materials with Cobre of 1.5 - 2.0 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Cromo | 0.05 % Show Material materials with Cromo of 0.05 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Hierro | 0.15 % Show Material materials with Hierro of 0.15 % | T7451 | WL 3.4394 | Plate |
0.15 % Show Material materials with Hierro of 0.15 % | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | |
Magnesio | 2.1 - 2.6 % Show Material materials with Magnesio of 2.1 - 2.6 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Níquel | 0.05 % Show Material materials with Níquel of 0.05 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Silicona | 0.12 % Show Material materials with Silicona of 0.12 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Titanio | 0.06 % Show Material materials with Titanio of 0.06 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Zinc | 5.7 - 6.7 % Show Material materials with Zinc of 5.7 - 6.7 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |