General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.82 g/cm³ Show Material materials with Densidad of 2.82 g/cm³ | T3 | EN 573-3, EN 754 | Rod, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 90.0 [-] Show Material materials with Dureza Brinell of 90.0 [-] | T3 | EN 573-3 | Rod, Tube | |
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T3 | EN 573-3, EN 754 | Rod, Tube | A50 | |
8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3, EN 754 | Rod, Tube | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3, EN 754 | Rod, Tube | A100 | ||
10.0 % Show Material materials with Elongación of 10.0 % | T3 | EN 573-3, EN 754 | Rod, Tube | A100 | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T3 | EN 573-3 | Tube | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3 | Tube | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T3 | EN 573-3 | Rod, Tube | ||
Módulo de cizallamiento | 26.0 - 27.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Módulo elástico | 70.0 - 73.0 GPa Show Material materials with Módulo elástico of 70.0 - 73.0 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Resistencia a la tracción | 280.0 MPa Show Material materials with Resistencia a la tracción of 280.0 MPa | T3 | EN 573-3, EN 754 | Rod, Tube | ||
290.0 MPa Show Material materials with Resistencia a la tracción of 290.0 MPa | T3 | EN 573-3, EN 754 | Rod, Tube | |||
300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | T3 | EN 573-3, EN 754 | Rod, Tube | |||
310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T3 | EN 573-3, EN 754 | Rod, Tube | |||
320.0 MPa Show Material materials with Resistencia a la tracción of 320.0 MPa | T3 | EN 573-3, EN 754 | Rod, Tube | |||
20.0 °C | 280.0 MPa Show Material materials with Resistencia a la tracción of 280.0 MPa | T3 | EN 573-3 | Rod | ||
20.0 °C | 290.0 MPa Show Material materials with Resistencia a la tracción of 290.0 MPa | T3 | EN 573-3 | Tube | ||
20.0 °C | 300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | T3 | EN 573-3 | Rod | ||
20.0 °C | 310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T3 | EN 573-3 | Tube | ||
20.0 °C | 320.0 MPa Show Material materials with Resistencia a la tracción of 320.0 MPa | T3 | EN 573-3 | Rod |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 816.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Coeficiente de dilatación térmica | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Conductividad térmica | 112.0 - 251.0 W/(m·K) Show Material materials with Conductividad térmica of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Temperatura de fusión | 500.0 - 650.0 °C Show Material materials with Temperatura de fusión of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 30000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
Resistividad eléctrica | 3.4e-08 - 6e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bismuto | 0.2 - 0.6 % Show Material materials with Bismuto of 0.2 - 0.6 % | T3 | EN 573-3, EN 754 | Rod, Tube |
Cobre | 4.5 - 6.0 % Show Material materials with Cobre of 4.5 - 6.0 % | T3 | EN 573-3, EN 754 | Rod, Tube |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T3 | EN 573-3 | Rod, Tube |
0.50 % Show Material materials with Hierro of 0.50 % | T3 | EN 573-3, EN 754 | Rod, Tube | |
Plomo | 0.2 - 0.6 % Show Material materials with Plomo of 0.2 - 0.6 % | T3 | EN 573-3, EN 754 | Rod, Tube |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | T3 | EN 573-3, EN 754 | Rod, Tube |
Zinc | 0.3 % Show Material materials with Zinc of 0.3 % | T3 | EN 573-3, EN 754 | Rod, Tube |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |