General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20.0 °C | 4.505 g/cm³ Show Material materials with Densidad of 4.505 g/cm³ | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.361 [-] Show Material materials with Coeficiente de Poisson of 0.361 [-] | Typical for Pure Titanium | ||||
Dureza Brinell | 20.0 °C | 150.0 Show Material materials with Dureza Brinell of 150.0 | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | |
20.0 °C | 150.0 Show Material materials with Dureza Brinell of 150.0 | Annealed | DIN 17864, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17860 | Forging | Transverse | |
Elongación | 20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging | Transverse |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | Annealed | WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
20.0 °C | 22.0 % Show Material materials with Elongación of 22.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Welded Tube, Wire, Sheet | ||
Estricción | 20.0 °C | 30.0 % Show Material materials with Estricción of 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging | Transverse |
20.0 °C | 30.0 % Show Material materials with Estricción of 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Módulo de cizallamiento | 20.0 °C | 45.0 GPa Show Material materials with Módulo de cizallamiento of 45.0 GPa | Annealed | WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Módulo elástico | 20.0 °C | 110.0 GPa Show Material materials with Módulo elástico of 110.0 GPa | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | |
200.0 °C | 97.0 GPa Show Material materials with Módulo elástico of 97.0 GPa | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | ||
400.0 °C | 82.0 GPa Show Material materials with Módulo elástico of 82.0 GPa | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | ||
Resistencia a la tracción | 20.0 °C | 390.0 - 540.0 MPa Show Material materials with Resistencia a la tracción of 390.0 - 540.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Welded Tube, Wire, Sheet | |
20.0 °C | 390.0 - 540.0 MPa Show Material materials with Resistencia a la tracción of 390.0 - 540.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging | Transverse | |
20.0 °C | 470.0 MPa Show Material materials with Resistencia a la tracción of 470.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
100.0 °C | 370.0 MPa Show Material materials with Resistencia a la tracción of 370.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
200.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
300.0 °C | 190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 520.0 J/(kg·K) Show Material materials with Calor específico of 520.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | |
200.0 °C | 570.0 J/(kg·K) Show Material materials with Calor específico of 570.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | ||
400.0 °C | 630.0 J/(kg·K) Show Material materials with Calor específico of 630.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | ||
Coeficiente de dilatación térmica | 8.400000000000001e-06 - 8.599999999999999e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 8.400000000000001e-06 - 8.599999999999999e-06 1/K | Typical for Pure Titanium | ||||
Conductividad térmica | 20.0 °C | 22.6 W/(m·K) Show Material materials with Conductividad térmica of 22.6 W/(m·K) | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | |
200.0 °C | 20.9 W/(m·K) Show Material materials with Conductividad térmica of 20.9 W/(m·K) | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | ||
400.0 °C | 19.3 W/(m·K) Show Material materials with Conductividad térmica of 19.3 W/(m·K) | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | ||
Temperatura de fusión | 1670.0 °C Show Material materials with Temperatura de fusión of 1670.0 °C | Typical for Pure Titanium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Resistividad eléctrica | 20.0 °C | 4.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.8e-07 Ω·m | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet |
200.0 °C | 8e-07 Ω·m Show Material materials with Resistividad eléctrica of 8e-07 Ω·m | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet | |
400.0 °C | 1.14e-06 Ω·m Show Material materials with Resistividad eléctrica of 1.14e-06 Ω·m | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbono | 0.06 Show Material materials with Carbono of 0.06 | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat |
0.08 Show Material materials with Carbono of 0.08 | Annealed | WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Hidrógeno | 0.013 Show Material materials with Hidrógeno of 0.013 | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet |
Hierro | 0.2 Show Material materials with Hierro of 0.2 | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat |
0.25 Show Material materials with Hierro of 0.25 | Annealed | WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Nitrógeno | 0.05 Show Material materials with Nitrógeno of 0.05 | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat |
0.06 Show Material materials with Nitrógeno of 0.06 | Annealed | WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Oxígeno | 0.18 Show Material materials with Oxígeno of 0.18 | Annealed | VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Welded Tube, Flat |
0.25 Show Material materials with Oxígeno of 0.25 | Annealed | WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Titanio | 98.7 % Show Material materials with Titanio of 98.7 % | Annealed | WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet |
99.1 % Show Material materials with Titanio of 99.1 % | Annealed | DIN 17850, VdTÜV WB 230-2, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Tube, Forging, Rod, Welded Tube, Wire, Flat |