General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Densidad | 20.0 °C | 2.65 g/cm³ Show Material materials with Densidad of 2.65 g/cm³ | T1 | DIN 1725-2, EN 1676, EN 1706 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 4xx.x Series Aluminium | |||
Dureza Brinell | 20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | T1 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 45.0 - 60.0 [-] Show Material materials with Dureza Brinell of 45.0 - 60.0 [-] | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 50.0 - 65.0 [-] Show Material materials with Dureza Brinell of 50.0 - 65.0 [-] | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
Elongación | 20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T1 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 6.0 - 12.0 % Show Material materials with Elongación of 6.0 - 12.0 % | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
Módulo elástico | 20.0 °C | 75.0 GPa Show Material materials with Módulo elástico of 75.0 GPa | T1 | DIN 1725-2, EN 1676, EN 1706 | |
Resistencia a la tracción | 20.0 °C | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | T1 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 150.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 150.0 - 200.0 MPa | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 160.0 MPa Show Material materials with Resistencia a la tracción of 160.0 MPa | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 170.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 230.0 MPa | T1 | DIN 1725-2, EN 1676, EN 1706 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | T1 | DIN 1725-2, EN 1676, EN 1706 | |
Coeficiente de dilatación térmica | 200.0 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T1 | DIN 1725-2, EN 1676, EN 1706 | |
Conductividad térmica | 20.0 °C | 130.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 190.0 W/(m·K) | T1 | DIN 1725-2, EN 1676, EN 1706 | |
Temperatura de fusión | 565.0 - 630.0 °C Show Material materials with Temperatura de fusión of 565.0 - 630.0 °C | Typical for Cast 4xx.x Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 17000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 26000000.0 S/m | T1 | DIN 1725-2, EN 1676, EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 85.1 % Show Material materials with Aluminio of 85.1 % | T1 | DIN 1725-2, EN 1676, EN 1706 |
Cobre | 0.05 Show Material materials with Cobre of 0.05 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Hierro | 0.5 Show Material materials with Hierro of 0.5 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Magnesio | 0.05 Show Material materials with Magnesio of 0.05 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Manganeso | 0.001 - 0.4 % Show Material materials with Manganeso of 0.001 - 0.4 % | T1 | DIN 1725-2, EN 1676, EN 1706 |
Silicona | 10.5 - 13.5 % Show Material materials with Silicona of 10.5 - 13.5 % | T1 | DIN 1725-2, EN 1676, EN 1706 |
Titanio | 0.15 Show Material materials with Titanio of 0.15 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.1 Show Material materials with Zinc of 0.1 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Processing methods | permanent mould casting, sample taken from casting or cast on |