General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |
2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
20.0 °C | 2.71 - 2.72 g/cm³ Show Material materials with Densidad of 2.71 - 2.72 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube |
Medidas
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Espesor | 60 mm Show Material materials with Espesor of 60 mm | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | 60 mm | Coil, Sheet, Foil |
400 mm Show Material materials with Espesor of 400 mm | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | 400 mm | Coil, Sheet, Foil |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 50.0 MPa Show Material materials with Bending Fatigue Strength of 50.0 MPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Dureza Brinell | 37.0 [-] Show Material materials with Dureza Brinell of 37.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 30.0 [-] Show Material materials with Dureza Brinell of 30.0 [-] | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 37.0 [-] Show Material materials with Dureza Brinell of 37.0 [-] | H14 | EN 573-3 | Rod, Flat, Tube | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
1 % Show Material materials with Elongación of 1 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | A50 | ||
2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Flat | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Flat | Transverse | |
Límite elástico | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | |
95.0 MPa Show Material materials with Límite elástico of 95.0 MPa | H14 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
95.0 - 150.0 MPa Show Material materials with Límite elástico of 95.0 - 150.0 MPa | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |||
20.0 °C | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | H14 | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | H14 | EN 573-3 | Flat | RP02 | |
20.0 °C | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | H14 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 95.0 MPa Show Material materials with Límite elástico of 95.0 MPa | H14 | EN 573-3 | Foil, Flat | RP02 | |
20.0 °C | 95.0 MPa Show Material materials with Límite elástico of 95.0 MPa | H14 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 100.0 MPa Show Material materials with Límite elástico of 100.0 MPa | H14 | EN 573-3 | Foil | RP02 | |
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |||
20.0 °C | 24.0 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 24.0 - 25.9 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 25.9 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 25.9 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 25.9 - 26.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Módulo elástico of 60.0 - 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Módulo elástico of 65.0 - 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Resistencia a la tracción | 105.0 - 170.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 170.0 MPa | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
20.0 °C | 105.0 - 155.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 155.0 MPa | H14 | EN 573-3, EN 683 | Foil, Flat, Strip, Sheet, Plate, Bar, Rod, Tube | ||
20.0 °C | 105.0 - 155.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 155.0 MPa | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 110.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 110.0 - 145.0 MPa | H14 | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 110.0 - 160.0 MPa Show Material materials with Resistencia a la tracción of 110.0 - 160.0 MPa | H14 | EN 573-3 | Foil | ||
20.0 °C | 115.0 - 155.0 MPa Show Material materials with Resistencia a la tracción of 115.0 - 155.0 MPa | H14 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 115.0 - 155.0 MPa Show Material materials with Resistencia a la tracción of 115.0 - 155.0 MPa | H14 | EN 573-3 | Flat | Transverse | |
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 898.0 J/(kg·K) Show Material materials with Calor específico of 898.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Coeficiente de dilatación térmica | -50 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | |
-50.0 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
100.0 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | 20-100°C | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.44e-05 1/K | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.54e-05 1/K | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Conductividad térmica | 138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Conductividad térmica of 205.0 - 210.0 W/(m·K) | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20.0 °C | 205.0 - 225.0 W/(m·K) Show Material materials with Conductividad térmica of 205.0 - 225.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 210.0 - 225.0 W/(m·K) Show Material materials with Conductividad térmica of 210.0 - 225.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 225.0 W/(m·K) Show Material materials with Conductividad térmica of 225.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Temperatura de fusión | 644.0 - 657.0 °C Show Material materials with Temperatura de fusión of 644.0 - 657.0 °C | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 33000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 33000000.0 - 34000000.0 S/m | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Conductividad eléctrica of 34400000.0 - 35500000.0 S/m | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Resistividad eléctrica | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.94e-08 - 3.03e-08 Ω·m | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
4.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.9e-08 Ω·m | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
20.0 °C | 2.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.95e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminio | 99.0 % Show Material materials with Aluminio of 99.0 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
0.05 % Show Material materials with Cobre of 0.05 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
Hierro | 1 % Show Material materials with Hierro of 1 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | Si + Fe |
Manganeso | 0.05 % Show Material materials with Manganeso of 0.05 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
0.05 % Show Material materials with Manganeso of 0.05 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |
Silicona | 1 % Show Material materials with Silicona of 1 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | Si + Fe |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
0.05 % Show Material materials with Titanio of 0.05 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
0.1 % Show Material materials with Zinc of 0.1 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels; Electronic devices: Housing of devices; Heat exchangers: Fins; Cable wrapping: Electric cable wrapping; Insulation; Solar: Solar collectors; Semi-rigid and corrugated: Smooth wall | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Welding | Excellent | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12) |