General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.84 g/cm³ Show Material materials with Densidad of 2.84 g/cm³ | T6 | WL 3.1754 | Casting | |
20.0 °C | 2.84 g/cm³ Show Material materials with Densidad of 2.84 g/cm³ | T6 | WL 3.1854, WL 3.1754 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 2xx.x Series Aluminium | ||||
Dureza Brinell | 80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | T6 | WL 3.1754 | Casting | ||
20.0 °C | 80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | T6 | WL 3.1854, WL 3.1754 | |||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | T6 | WL 3.1754 | Casting | A50 | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | T6 | WL 3.1854, WL 3.1754 | |||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T6 | WL 3.1754 | Casting | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T6 | WL 3.1854, WL 3.1754 | |||
Resistencia a la tracción | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | T6 | WL 3.1754 | Casting | ||
190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | T6 | WL 3.1754 | Casting | |||
20.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | T6 | WL 3.1854, WL 3.1754 | |||
20.0 °C | 185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | T6 | WL 3.1854, WL 3.1754 | |||
20.0 °C | 190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | T6 | WL 3.1854, WL 3.1754 | |||
20.0 °C | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | T6 | WL 3.1854, WL 3.1754 | |||
20.0 °C | 215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | T6 | WL 3.1854, WL 3.1754 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 875.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 875.0 - 963.0 J/(kg·K) | Typical for Cast 2xx.x Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 1.9999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9999999999999998e-05 1/K | T6 | WL 3.1754 | Casting | |
100 °C | 1.9999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9999999999999998e-05 1/K | T6 | WL 3.1754 | Casting | ||
Conductividad térmica | 155 W/(m·K) Show Material materials with Conductividad térmica of 155 W/(m·K) | T6 | WL 3.1754 | Casting | ||
20.0 °C | 155.0 W/(m·K) Show Material materials with Conductividad térmica of 155.0 W/(m·K) | T6 | WL 3.1854, WL 3.1754 | |||
Temperatura de fusión | 510.0 - 790.0 °C Show Material materials with Temperatura de fusión of 510.0 - 790.0 °C | Typical for Cast 2xx.x Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 21000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 S/m | T6 | WL 3.1754 | Casting | |
20.0 °C | 21000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 S/m | T6 | WL 3.1854, WL 3.1754 | ||
Resistividad eléctrica | 4.76e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 Ω·m | T6 | WL 3.1754 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 93.4 % Show Material materials with Aluminio of 93.4 % | T6 | WL 3.1854, WL 3.1754 | |
Circonio | 0.1 - 0.3 % Show Material materials with Circonio of 0.1 - 0.3 % | T6 | WL 3.1754 | Casting |
Cobre | 4.2 - 5.0 % Show Material materials with Cobre of 4.2 - 5.0 % | T6 | WL 3.1854, WL 3.1754 | |
4.5 - 5.5 % Show Material materials with Cobre of 4.5 - 5.5 % | T6 | WL 3.1754 | Casting | |
Hierro | 0.35 % Show Material materials with Hierro of 0.35 % | T6 | WL 3.1854, WL 3.1754 | |
0.50 % Show Material materials with Hierro of 0.50 % | T6 | WL 3.1754 | Casting | |
Magnesio | 0.15 - 0.35 % Show Material materials with Magnesio of 0.15 - 0.35 % | T6 | WL 3.1854, WL 3.1754 | |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | T6 | WL 3.1854, WL 3.1754 | |
0.2 - 0.3 % Show Material materials with Manganeso of 0.2 - 0.3 % | T6 | WL 3.1754 | Casting | |
Níquel | 0.03 % Show Material materials with Níquel of 0.03 % | T6 | WL 3.1854, WL 3.1754 | |
1.3 - 1.8 % Show Material materials with Níquel of 1.3 - 1.8 % | T6 | WL 3.1754 | Casting | |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | T6 | WL 3.1854, WL 3.1754 | Casting |
Titanio | 0.15 - 0.25 % Show Material materials with Titanio of 0.15 - 0.25 % | T6 | WL 3.1854, WL 3.1754 | Casting |
Zinc | 0.1 Show Material materials with Zinc of 0.1 | T6 | WL 3.1854, WL 3.1754 |
Technological properties
Property | ||
---|---|---|
Processing methods | investment casting, sample taken from casting |