General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 8.89 g/cm³ Show Material materials with Density of 8.89 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | |
Elongation | 23.0 °C | 40 % Show Material materials with Elongation of 40 % | in 2 in. |
Hardness, Rockwell B | 23.0 °C | 80 [-] Show Material materials with Hardness, Rockwell B of 80 [-] | |
Tensile strength | 23.0 °C | 449 MPa Show Material materials with Tensile strength of 449 MPa | |
Yield strength | 23.0 °C | 138 MPa Show Material materials with Yield strength of 138 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K | from 30°C to the mentioned temperature |
Melting point | 1440 °C Show Material materials with Melting point of 1440 °C | ||
Specific heat capacity | 23.0 °C | 452 J/(kg·K) Show Material materials with Specific heat capacity of 452 J/(kg·K) | |
Thermal conductivity | 23.0 °C | 86 W/(m·K) Show Material materials with Thermal conductivity of 86 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 23.0 °C | 7.5E-8 Ω·m Show Material materials with Electrical resistivity of 7.5E-8 Ω·m |
Magnetic
Property | Value |
---|---|
Curie temperature | 360 °C Show Material materials with Curie temperature of 360 °C |
Chemical properties
Property | Value |
---|---|
Carbon | 0.02 % Show Material materials with Carbon of 0.02 % |
Cobalt | 1E-3 % Show Material materials with Cobalt of 1E-3 % |
Iron | 5E-3 % Show Material materials with Iron of 5E-3 % |
Nickel | 99.97 % Show Material materials with Nickel of 99.97 % |
Silicon | 1E-3 % Show Material materials with Silicon of 1E-3 % |
Sulfur | 1E-3 % Show Material materials with Sulfur of 1E-3 % |
Technological properties
Property | ||
---|---|---|
Application areas | Common applications of Nickel 270: Anode plates, hydrogen thyratron components, passive cathodes, cathodes shanks, plater bars, transistor enclosures |