Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 8.2 g/cm³ Show Material materials with Density of 8.2 g/cm³ |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 200.0 °C | 9.5E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.5E-6 1/K |
400.0 °C | 1.01E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.01E-5 1/K | |
600.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | |
800.0 °C | 1.13E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.13E-5 1/K | |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 23.0 °C | 4.2E-7 Ω·m Show Material materials with Electrical resistivity of 4.2E-7 Ω·m |
Magnetic
Property | Temperature | Value | Comment |
---|---|---|---|
Coercive force | 843.0 °C | 318 A/m Show Material materials with Coercive force of 318 A/m | at 2.3T |
870.0 °C | 200 A/m Show Material materials with Coercive force of 200 A/m | at 2.3T | |
885.0 °C | 56 A/m Show Material materials with Coercive force of 56 A/m | at 2.3T | |
Curie temperature | 932 °C Show Material materials with Curie temperature of 932 °C | ||
Relative magnetic permeability | 843.0 °C | 2000 [-] Show Material materials with Relative magnetic permeability of 2000 [-] | |
870.0 °C | 2650 [-] Show Material materials with Relative magnetic permeability of 2650 [-] | ||
885.0 °C | 10000 [-] Show Material materials with Relative magnetic permeability of 10000 [-] | ||
Saturation induction | 23.0 °C | 2.3 T Show Material materials with Saturation induction of 2.3 T | at 19.9A/m |
Saturation magnetostriction | 23.0 °C | 6E-5 [-] Show Material materials with Saturation magnetostriction of 6E-5 [-] |
Chemical properties
Property | Value |
---|---|
Carbon | 0.01 % Show Material materials with Carbon of 0.01 % |
Cobalt | 48.75 % Show Material materials with Cobalt of 48.75 % |
Iron | balance |
Manganese | 0.05 % Show Material materials with Manganese of 0.05 % |
Silicon | 0.05 % Show Material materials with Silicon of 0.05 % |
Vanadium | 1.95 % Show Material materials with Vanadium of 1.95 % |
Technological properties
Property | ||
---|---|---|
Application areas | Instruments, Radar, Radio transformers etc |