Abmessung
Property | Value |
---|---|
Breite | 950 - 1100 mm Show Supplier Material materials with Breite of 950 - 1100 mm |
Dicke | 120 - 600 mm Show Supplier Material materials with Dicke of 120 - 600 mm |
Mechanisch
Property | Value | Comment |
---|---|---|
Härte, Brinell | 365 - 410 [-] Show Supplier Material materials with Härte, Brinell of 365 - 410 [-] | as-delivered condition |
Härte, Rockwell C | 28 - 51 [-] Show Supplier Material materials with Härte, Rockwell C of 28 - 51 [-] | |
Zugfestigkeit | 1220 - 1385 MPa Show Supplier Material materials with Zugfestigkeit of 1220 - 1385 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100 °C | 1.11e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.11e-05 1/K | for 20°C to the mentioned temperature |
200 °C | 1.29e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.29e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.34e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.34e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.35e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.35e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.38e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.38e-05 1/K | for 20°C to the mentioned temperature | |
600 °C | 1.41e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.41e-05 1/K | for 20°C to the mentioned temperature | |
700 °C | 1.43e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.43e-05 1/K | for 20°C to the mentioned temperature | |
Wärmeleitfähigkeit | 23 °C | 36 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 36 W/(m·K) | |
150 °C | 37.4 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 37.4 W/(m·K) | ||
300 °C | 33 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 33 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Andere | Plus additions |
Chrom | 1.9 % Show Supplier Material materials with Chrom of 1.9 % |
Eisen | Balance |
Kohlenstoff | 0.36 % Show Supplier Material materials with Kohlenstoff of 0.36 % |
Mangan | 0.9 % Show Supplier Material materials with Mangan of 0.9 % |
Molybdän | 0.5 % Show Supplier Material materials with Molybdän of 0.5 % |
Nickel | 0.5 % Show Supplier Material materials with Nickel of 0.5 % |
Silizium | 0.4 % Show Supplier Material materials with Silizium of 0.4 % |
Technological properties
Property | ||
---|---|---|
Application areas | Plastic injection and extrusion moulds for all dimensions and deep engraving with high demands on polishability, wear resistance and core strength. | |
Heat Treatment | Soft annealing: 710-740°C (Cooling in furnace) - Hardening: 820-850°C and quenching in oil or polymer |