Allgemein
Property | Value | Comment | |
---|---|---|---|
Carbon equivalent (CET) | 0.22 [-] Show Supplier Material materials with Carbon equivalent (CET) of 0.22 [-] | typ. value for thickness 8 ≤ t ≤ 100 mm | |
0.23 [-] Show Supplier Material materials with Carbon equivalent (CET) of 0.23 [-] | typ. value for thickness 100 ≤ t ≤ 150 mm | ||
Carbon equivalent (CEV) | 0.39 [-] Show Supplier Material materials with Carbon equivalent (CEV) of 0.39 [-] | typ. value for thickness 8 ≤ t ≤ 100 mm | |
0.4 [-] Show Supplier Material materials with Carbon equivalent (CEV) of 0.4 [-] | typ. value for thickness 100 < t ≤ 150 mm | ||
0.42 [-] Show Supplier Material materials with Carbon equivalent (CEV) of 0.42 [-] | max. value for thickness 8 ≤ t ≤ 100 mm | ||
0.45 [-] Show Supplier Material materials with Carbon equivalent (CEV) of 0.45 [-] | max. value for thickness 100 ≤ t ≤ 150 mm | ||
0.52 [-] Show Supplier Material materials with Carbon equivalent (CEV) of 0.52 [-] | max. value for thickness 8 ≤ t ≤ 100 mm and 100 < t ≤ 150 mm according to EN 10025-5 | ||
Carbon equivalent note | CEV = C + Mn/6 + (Cr+Mo+V)/5 + (Cu+Ni)/15 and CET = C + (Mn+Mo)/10 + (Cr+Cu)/20 + Ni/40 |
Mechanisch
Property | Temperature | Value | Testing Standard | Comment |
---|---|---|---|---|
Charpy impact energy, V-notch | -50 °C | 19 J Show Supplier Material materials with Charpy impact energy, V-notch of 19 J | EN ISO 148-1 | Option 2 | single value | longitudinal specimen |
-50 °C | 27 J Show Supplier Material materials with Charpy impact energy, V-notch of 27 J | EN ISO 148-1 | Option 2 | average of 3 tests | longitudinal specimen | |
-20 °C | 28 J Show Supplier Material materials with Charpy impact energy, V-notch of 28 J | EN ISO 148-1 | single value | longitudinal specimen | |
-20 °C | 40 J Show Supplier Material materials with Charpy impact energy, V-notch of 40 J | EN ISO 148-1 | average of 3 tests | longitudinal specimen | |
Dehnung | 18 % Show Supplier Material materials with Dehnung of 18 % | EN ISO 6892-1 | min. for plate thickness 63 < t ≤ 150 mm | transverse specimens, A5 | |
19 % Show Supplier Material materials with Dehnung of 19 % | EN ISO 6892-1 | min. for plate thickness 40 < t ≤ 63 mm | transverse specimens, A5 | ||
20 % Show Supplier Material materials with Dehnung of 20 % | EN ISO 6892-1 | min. for plate thickness up to 40 mm | transverse specimens, A5 | ||
Streckgrenze | 295 MPa Show Supplier Material materials with Streckgrenze of 295 MPa | EN ISO 6892-1 | min. ReH for plate thickness 100 < t ≤ 150 mm | transverse specimens | |
315 MPa Show Supplier Material materials with Streckgrenze of 315 MPa | EN ISO 6892-1 | min. ReH for plate thickness 80 < t ≤ 100 mm | transverse specimens | ||
325 MPa Show Supplier Material materials with Streckgrenze of 325 MPa | EN ISO 6892-1 | min. ReH for plate thickness 63 < t ≤ 80 mm | transverse specimens | ||
335 MPa Show Supplier Material materials with Streckgrenze of 335 MPa | EN ISO 6892-1 | min. ReH for plate thickness 40 < t ≤ 63 mm | transverse specimens | ||
345 MPa Show Supplier Material materials with Streckgrenze of 345 MPa | EN ISO 6892-1 | min. ReH for plate thickness 16 < t ≤ 40 mm | transverse specimens | ||
355 MPa Show Supplier Material materials with Streckgrenze of 355 MPa | EN ISO 6892-1 | min. ReH for plate thickness t ≤ 16 mm | transverse specimens | ||
Zugfestigkeit | 450 - 600 MPa Show Supplier Material materials with Zugfestigkeit of 450 - 600 MPa | EN ISO 6892-1 | for plate thickness 100 < t ≤ 150 mm | transverse specimens | |
470 - 630 MPa Show Supplier Material materials with Zugfestigkeit of 470 - 630 MPa | EN ISO 6892-1 | for plate thickness up to 100 mm | transverse specimens |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminium | 0.02 % Show Supplier Material materials with Aluminium of 0.02 % | min. | |
Chrom | 0.4 - 0.6 % Show Supplier Material materials with Chrom of 0.4 - 0.6 % | ||
Eisen | Balance | ||
Kohlenstoff | 0.08 % Show Supplier Material materials with Kohlenstoff of 0.08 % | max. | |
Kupfer | 0.25 - 0.4 % Show Supplier Material materials with Kupfer of 0.25 - 0.4 % | ||
Mangan | 1.4 % Show Supplier Material materials with Mangan of 1.4 % | max. | |
Molybdän | 0.08 % Show Supplier Material materials with Molybdän of 0.08 % | max. | |
Nickel | 0.5 % Show Supplier Material materials with Nickel of 0.5 % | max. | |
Niobium | 0.05 % Show Supplier Material materials with Niobium of 0.05 % | max. | |
Phosphor | 0.02 % Show Supplier Material materials with Phosphor of 0.02 % | max. | |
Schwefel | 0.002 % Show Supplier Material materials with Schwefel of 0.002 % | max. | |
Silizium | 0.45 % Show Supplier Material materials with Silizium of 0.45 % | max. | |
Stickstoff | 0.01 % Show Supplier Material materials with Stickstoff of 0.01 % | max. | |
Titan | 0.015 % Show Supplier Material materials with Titan of 0.015 % | max. | |
Vanadium | 0.01 % Show Supplier Material materials with Vanadium of 0.01 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | The steel can especially be used in steel constructions for bridges and high rise buildings where weathering steel with good weldability is demanded. | |
Cold Forming | DIWETEN 355+M can be cold formed, i.e. forming at temperatures below 580 °C, as any comparable structural steel in accordance with EN 10025. Cold forming is always related to a hardening of the steel and to a decrease in toughness. This change in the mechanical properties can in general be partially recovered through a subsequent stress relief heat treatment. Flame cut or sheared edges in the bending area should be ground before cold forming. For larger cold forming degrees we recommend consulting us prior to ordering. | |
Corrosion properties | Atmospheric corrosion resistance means that the steel - due to the chemical composition - presents a higher resistance against atmospheric corrosion in comparison to unalloyed steels because a protective coating which protects the surface and decelerates the normal corrosion process is formed on the surface and influenced by the weather. This property is defined by the weather resistance index I > 6.0 in accordance with ASTM G101. Generally, the corrosion velocity decreases with increasing service life. Even after the formation of the patina, a total stop of the corrosion process is not achieved. However, the patina offers - in comparison to unalloyed steels - a better protection against atmospheric corrosion in industrial, city or rural atmosphere, which enables the application of uncoated steels under certain circumstances. Initial formation, time of development and protective effect of the patina on steels with improved atmospheric corrosion resistance are extremely depending on the constructional design and the atmospheric and environmental conditions in the respective case. In any case, usual constructional standards for the construction with steels with improved atmospheric corrosion resistance are to be observed, as i.e. the German guideline DASt 007 (“Delivery, fabrication and application of steels with improved atmospheric corrosion resistance”). In addition, the weather resistance I-index > 6.0 in accordance with ASTM G101-04 (2015) is valid. I = 26.01 · (% Cu) + 3.88 · (% Ni) + 1.2 · (% Cr) + 1.49 · (% Si) + 17.28 · (% P) – 7.29 · (% Cu) · (% Ni) - 9.10 · (% Ni) · (% P) – 33.39 · (% Cu) | |
Delivery condtion | Thermomechanically rolled (short designation +M). General technical delivery requirements: Unless otherwise agreed, the general technical delivery requirements in accordance with EN 10021 apply. | |
Flame cutting and welding | DIWETEN 355+M has despite its weathering property a good weldability if the general technical rules (see EN 1011) are respected.. However the hardenability of the steel is increased due to the Cu and Cr alloying. Owing to the low carbon content oxygen cutting, plasma and laser cutting can be carried out up to large thickness without preheating. The preheat conditions during welding have to be adapted to the slightly increased carbon equivalent compared to non-weathering thermomechanically rolled steels. If necessary, the corrosion resistance of the welding deposit has to be assured by selection of adequate weld metals or other anti-corrosion measures. | |
General note | If particular requirements, which are not covered in this material data sheet, are to be met by the steel due to its intended use or processing, these requirements are to be agreed before placing the order. The information in this technical data sheet is a product description. This material data sheet is updated at irregular intervals. The current version is available from the mill or as download at www.dillinger.de. | |
Heat Treatment | Welded joints of DIWETEN 355+M are usually used in welded condition. If a stress relief heat treatment is necessary, it is carried out in the temperature range between 530 and 580 °C with cooling in air. The holding time should not exceed 4 hours (even if multiple operations are carried out). For particular heat treatment requirements we recommend consulting us prior to ordering. | |
Hot forming | Hot forming, i.e. forming at temperatures above 580 °C, leads to changes in the original material condition. It is impossible to re-establish the same material properties that had been achieved during the original manufacture through a further treatment. Therefore hot forming is not permitted. | |
Options | 1) Tensile and impact test on each mother plate, 2) Supplementary Charpy-V-test: absorbed energy KV2 27 J at -50 °C as the average of 3 tests and minimum single value of 19 J, applicable in the sense of S355J5W+M. | |
Other | DIWETEN 355+M can be delivered in thicknesses from 8 to 150 mm according to Dillinger delivery program. | |
Processing methods | The entire processing and application techniques are of fundamental importance to the reliability of the parts and assemblies made from this steel. The user should ensure that his design, construction and processing methods are aligned with the material, correspond to the state-of-the-art that the fabricator has to comply with and are suitable for the intended use. The customer is responsible for the selection of the material. The recommendations in accordance with EN 1011-2, guideline DASt 007, SEW 088 as well as recommendations regarding job safety in accordance with national rules should be observed. | |
Surface condition | Surface quality: Unless otherwise agreed, the specifications will be in accordance with EN 10163-2, class A2. | |
Testings | Ultrasonic testing: Unless otherwise agreed, DIWETEN 355+M meets the requirements of class S1E1 according to EN 10160. Tensile test at ambient temperature – transverse test specimens Tensile test and impact tests are carried out with respect to EN 10025-5 once per heat, 60 t and thickness range as specified for the yield strength. Tests on every mother plate are possible on request. The test pieces are taken and prepared according to parts 1 and 5 of EN 10025. The tensile test is carried out on specimens of gauge length Lo = 5.65⋅√So respectively Lo = 5⋅do, in accordance with EN ISO 6892-1. Unless otherwise agreed, the impact test is carried out at -20 °C (at -50 °C for option 2) on longitudinal Charpy-V-specimens using a 2 mm striker in accordance with EN ISO 148-1. Unless otherwise agreed, the test results are documented in a certificate 3.1 in accordance with EN 10204. | |
Tolerances | Unless otherwise agreed, tolerances are in accordance with 10029, with class A for the thickness. |