Allgemein
Property | Value | Comment |
---|---|---|
Coefficient of friction | 0.25 [-] Show Supplier Material materials with Coefficient of friction of 0.25 [-] | DIN 53375, B, Against dry running steel |
Dichte | 0.95 g/cm³ Show Supplier Material materials with Dichte of 0.95 g/cm³ | ISO 1183 |
Wasserabsorption | 0.01 % Show Supplier Material materials with Wasserabsorption of 0.01 % | max., ISO 62 |
Mechanisch
Property | Value | Comment | |
---|---|---|---|
Biegefestigkeit | 22 MPa Show Supplier Material materials with Biegefestigkeit of 22 MPa | ISO 178 | |
Dehnung | 700 % Show Supplier Material materials with Dehnung of 700 % | min., ISO 527 | |
Elastizitätsmodul | 1 GPa Show Supplier Material materials with Elastizitätsmodul of 1 GPa | ISO 527 | |
Elongation at yield | 9 % Show Supplier Material materials with Elongation at yield of 9 % | ISO 527 | |
Härte, Shore D | 64 [-] Show Supplier Material materials with Härte, Shore D of 64 [-] | DIN 53505 | |
Reißfestigkeit | 31 kN/m Show Supplier Material materials with Reißfestigkeit of 31 kN/m | ISO 527 | |
Schlagfestigkeit, Charpy gekerbt | 29 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 29 kJ/m² | ISO 179 | |
Streckgrenze | 22 MPa Show Supplier Material materials with Streckgrenze of 22 MPa | ISO 527 | |
Schlagzähigkeit, Charpy ungekerbt | No break, ISO 179 |
Thermisch
Property | Value | Pressure | Comment | ||
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 0.00015 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 0.00015 1/K | DIN 53752 | |||
Max. Betriebstemperatur | 90 °C Show Supplier Material materials with Max. Betriebstemperatur of 90 °C | Longterm | |||
Long | |||||
Short | |||||
Min. Betriebstemperatur | -50 °C Show Supplier Material materials with Min. Betriebstemperatur of -50 °C | Longterm | |||
Vicat-Erweichungstemperatur | 80 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 80 °C | ISO 306, VST B50 | |||
Wärmeformbeständigkeitstemperatur | 69 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 69 °C | 0.45 MPa | |||
Wärmeleitfähigkeit | 0.42 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 0.42 W/(m·K) | DIN 52612 | |||
Entflammbarkeit | HB UL 94 |
Elektrisch
Property | Value | Comment |
---|---|---|
Dielektrizitätskonstante | 2.35 [-] Show Supplier Material materials with Dielektrizitätskonstante of 2.35 [-] | DIN 53483 |
Durchschlagfestigkeit | 17 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 17 kV/mm | VDE 0303 |
Surface resistivity | 1e+16 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+16 Ω/sq | min., VDE 0303 |
Verlustfaktor | 0.0003 [-] Show Supplier Material materials with Verlustfaktor of 0.0003 [-] | DIN 53483 |
Volume resistivity | 1e+15 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+15 Ω·cm | min., VDE 0303 |
Technological properties
Property | ||
---|---|---|
Application areas | Cutting boards, linings and work benches | |
Certifications | Food Contact: FDA and EU 10/2011, RoHS,REACH | |
UV resistance | Partly |