Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 14.7 % Show Material materials with Dehnung of 14.7 % | Predicted Value, A80 | ||||
15.5 % Show Material materials with Dehnung of 15.5 % | Predicted Value, A200 | |||||
16.5 % Show Material materials with Dehnung of 16.5 % | Predicted Value, Transverse | |||||
17.8 % Show Material materials with Dehnung of 17.8 % | Predicted Value, A50 | |||||
17.8 % Show Material materials with Dehnung of 17.8 % | Predicted Value, A80 Transverse | |||||
18.4 % Show Material materials with Dehnung of 18.4 % | Predicted Value, A5 | |||||
20.9 % Show Material materials with Dehnung of 20.9 % | Predicted Value | |||||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 210 - 212 GPa Show Material materials with Elastizitätsmodul of 210 - 212 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 210 GPa Show Material materials with Elastizitätsmodul of 210 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 188 - 199 GPa Show Material materials with Elastizitätsmodul of 188 - 199 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 188 GPa Show Material materials with Elastizitätsmodul of 188 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Flächenreduzierung | 41.4 % Show Material materials with Flächenreduzierung of 41.4 % | Predicted Value, Transverse | ||||
47.2 % Show Material materials with Flächenreduzierung of 47.2 % | Predicted Value | |||||
Poissonzahl | 20 °C | 0.284 [-] Show Material materials with Poissonzahl of 0.284 [-] | normalized or normalized formed (+N) | EN 10084, ISO 683-3 | Bar, Flat, Forging, Wire | |
Scherfestigkeit | 514.2 MPa Show Material materials with Scherfestigkeit of 514.2 MPa | Predicted Value | ||||
Schubmodule | 20 °C | 81 GPa Show Material materials with Schubmodule of 81 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 1.1e-05 - 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1e-05 - 1.21e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 1.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 460 - 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 460 - 461 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 460 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 460 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Temperaturleitfähigkeit | 20 °C | 12.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.7 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
100 °C | 12 mm²/s Show Material materials with Temperaturleitfähigkeit of 12 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 11 mm²/s Show Material materials with Temperaturleitfähigkeit of 11 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 9.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.9 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 8.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.7 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 7.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.3 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 6 mm²/s Show Material materials with Temperaturleitfähigkeit of 6 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Wärmeleitfähigkeit | 20 °C | 42 - 45.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 - 45.9 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 45.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.9 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 39.8 - 46.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.8 - 46.4 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 39.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.8 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 46.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46.4 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 37.7 - 45.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.7 - 45.6 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 37.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.7 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 45.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.6 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 43.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.5 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 40.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.9 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.2 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 35.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.5 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 4 S/m Show Material materials with Elektrische Leitfähigkeit of 4 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 1.6e-07 - 2.27e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.6e-07 - 2.27e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 1.6e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.6e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 2.27e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.27e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 2.76e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.76e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 3.46e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.46e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 4.31e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.31e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 5.32e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.32e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 6.48e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.48e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 7.81e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.81e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.8 - 1.1 % Show Material materials with Chrom of 0.8 - 1.1 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Kohlenstoff | 0.14 - 0.19 % Show Material materials with Kohlenstoff of 0.14 - 0.19 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Kupfer | 0.4 % Show Material materials with Kupfer of 0.4 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Mangan | 1 - 1.3 % Show Material materials with Mangan of 1 - 1.3 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Schwefel | 0.035 % Show Material materials with Schwefel of 0.035 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Silizium | 0.15 - 0.4 % Show Material materials with Silizium of 0.15 - 0.4 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
0.4 % Show Material materials with Silizium of 0.4 % | normalized or normalized formed (+N) | EN 10084, ISO 683-3 | Bar, Flat, Forging, Wire |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |