EN 10088-1 Grade X2CrNiMoN17-13-3 solution annealed (+AT)

View suppliers (7)
Want to keep this datasheet? Save it now in your required format

Description

Material X2CrNiMoN17-13-3 is comparable to X 2 CrNiMoN 17 13 3 acc. to DIN17440 : 1985-07. It is a fully austenitic steel that is suitable for mirror finishing. It shows higher strength owing to nitrogen alloying and owing to more molybdenum addition higher corrosion resistance especially to non oxidizing acids and halogenated media than 1.4406. Resistance to intercrystalline corrosion in delivery condition as well as in sensitized condition. The material shows higher resistance to selective corrosion than 1.4435 and excellent limiting fatigue stres behavior also under chemical load. Furthermore it shows good cryogenic toughness. It is therefore suitable for refrigeration up to -270 °C.

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValue

Dichte

20.0 °C

8 - 8.01 g/cm³

Show Material materials with Dichte of 8 - 8.01 g/cm³

Mechanisch

PropertyTemperatureValue

Dehnung

20.0 °C

40 %

Show Material materials with Dehnung of 40 %

Dehnung A80, transversal

20.0 °C

35 - 40 %

Show Material materials with Dehnung A80, transversal of 35 - 40 %

Dehnung, transversal

20.0 °C

30 - 40 %

Show Material materials with Dehnung, transversal of 30 - 40 %

Elastizitätsmodul

-100.0 °C

206 GPa

Show Material materials with Elastizitätsmodul of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastizitätsmodul of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastizitätsmodul of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastizitätsmodul of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastizitätsmodul of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastizitätsmodul of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastizitätsmodul of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastizitätsmodul of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastizitätsmodul of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastizitätsmodul of 134 GPa

Hardness, Brinell, trans

20.0 °C

250 [-]

Show Material materials with Hardness, Brinell, trans of 250 [-]

Härte, Brinell

20.0 °C

250 [-]

Show Material materials with Härte, Brinell of 250 [-]

Poissonzahl

20.0 °C

0.28 [-]

Show Material materials with Poissonzahl of 0.28 [-]

Schubmodule

20.0 °C

77.3 GPa

Show Material materials with Schubmodule of 77.3 GPa

Streckgrenze Rp 0,2

20.0 °C

200 - 280 MPa

Show Material materials with Streckgrenze Rp 0,2 of 200 - 280 MPa

100.0 °C

211 - 215 MPa

Show Material materials with Streckgrenze Rp 0,2 of 211 - 215 MPa

150.0 °C

185 - 195 MPa

Show Material materials with Streckgrenze Rp 0,2 of 185 - 195 MPa

200.0 °C

167 - 175 MPa

Show Material materials with Streckgrenze Rp 0,2 of 167 - 175 MPa

250.0 °C

155 - 180 MPa

Show Material materials with Streckgrenze Rp 0,2 of 155 - 180 MPa

300.0 °C

145 - 170 MPa

Show Material materials with Streckgrenze Rp 0,2 of 145 - 170 MPa

350.0 °C

140 - 150 MPa

Show Material materials with Streckgrenze Rp 0,2 of 140 - 150 MPa

400.0 °C

135 - 145 MPa

Show Material materials with Streckgrenze Rp 0,2 of 135 - 145 MPa

450.0 °C

131 - 140 MPa

Show Material materials with Streckgrenze Rp 0,2 of 131 - 140 MPa

500.0 °C

129 - 138 MPa

Show Material materials with Streckgrenze Rp 0,2 of 129 - 138 MPa

550.0 °C

127 - 136 MPa

Show Material materials with Streckgrenze Rp 0,2 of 127 - 136 MPa

Unlock all property charts

Streckgrenze Rp 0,2, transversal

20.0 °C

200 - 300 MPa

Show Material materials with Streckgrenze Rp 0,2, transversal of 200 - 300 MPa

Streckgrenze Rp 1,0

20.0 °C

315 MPa

Show Material materials with Streckgrenze Rp 1,0 of 315 MPa

100.0 °C

245 - 246 MPa

Show Material materials with Streckgrenze Rp 1,0 of 245 - 246 MPa

150.0 °C

218 - 225 MPa

Show Material materials with Streckgrenze Rp 1,0 of 218 - 225 MPa

200.0 °C

198 - 205 MPa

Show Material materials with Streckgrenze Rp 1,0 of 198 - 205 MPa

250.0 °C

183 - 215 MPa

Show Material materials with Streckgrenze Rp 1,0 of 183 - 215 MPa

300.0 °C

175 - 205 MPa

Show Material materials with Streckgrenze Rp 1,0 of 175 - 205 MPa

350.0 °C

169 - 180 MPa

Show Material materials with Streckgrenze Rp 1,0 of 169 - 180 MPa

400.0 °C

164 - 175 MPa

Show Material materials with Streckgrenze Rp 1,0 of 164 - 175 MPa

450.0 °C

160 - 170 MPa

Show Material materials with Streckgrenze Rp 1,0 of 160 - 170 MPa

500.0 °C

158 - 168 MPa

Show Material materials with Streckgrenze Rp 1,0 of 158 - 168 MPa

550.0 °C

157 - 166 MPa

Show Material materials with Streckgrenze Rp 1,0 of 157 - 166 MPa

Unlock all property charts

Streckgrenze Rp 1,0, transversal

20.0 °C

315 - 330 MPa

Show Material materials with Streckgrenze Rp 1,0, transversal of 315 - 330 MPa

Zugfestigkeit

20.0 °C

580 - 800 MPa

Show Material materials with Zugfestigkeit of 580 - 800 MPa

Zugfestigkeit, transversal

20.0 °C

580 - 800 MPa

Show Material materials with Zugfestigkeit, transversal of 580 - 800 MPa

Thermisch

PropertyTemperatureValueComment

Koeffizient der thermischen Ausdehnung

-100.0 °C

1.49E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2E-5 1/K

Unlock all property charts

Max. Betriebstemperatur, lang

-270 - 0 °C

Show Material materials with Max. Betriebstemperatur, lang of -270 - 0 °C

Schmelzpunkt

1230 - 1480 °C

Show Material materials with Schmelzpunkt of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Spezifische Wärmekapazität

-100.0 °C

440 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 571 J/(kg·K)

Unlock all property charts

Temperaturleitfähigkeit

20.0 °C

3.6 mm²/s

Show Material materials with Temperaturleitfähigkeit of 3.6 mm²/s

100.0 °C

3.7 mm²/s

Show Material materials with Temperaturleitfähigkeit of 3.7 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4 mm²/s

300.0 °C

4.4 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4.4 mm²/s

400.0 °C

4.6 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4.6 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4.7 mm²/s

600.0 °C

4.9 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4.9 mm²/s

700.0 °C

5.2 mm²/s

Show Material materials with Temperaturleitfähigkeit of 5.2 mm²/s

800.0 °C

5.5 mm²/s

Show Material materials with Temperaturleitfähigkeit of 5.5 mm²/s

Unlock all property charts

Wärmeleitfähigkeit

20.0 °C

13.5 - 15 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 13.5 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 14.9 W/(m·K)

200.0 °C

16.7 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 16.7 W/(m·K)

300.0 °C

18.3 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 18.3 W/(m·K)

400.0 °C

19.8 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 19.8 W/(m·K)

500.0 °C

21.3 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 21.3 W/(m·K)

600.0 °C

22.7 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 22.7 W/(m·K)

700.0 °C

24.2 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 24.2 W/(m·K)

800.0 °C

25.6 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 25.6 W/(m·K)

Unlock all property charts

Elektrisch

PropertyTemperatureValue

spezifischer Widerstand

20.0 °C

7.5E-7 - 7.75E-7 Ω·m

Show Material materials with spezifischer Widerstand of 7.5E-7 - 7.75E-7 Ω·m

100.0 °C

8.42E-7 Ω·m

Show Material materials with spezifischer Widerstand of 8.42E-7 Ω·m

200.0 °C

9.04E-7 Ω·m

Show Material materials with spezifischer Widerstand of 9.04E-7 Ω·m

300.0 °C

9.62E-7 Ω·m

Show Material materials with spezifischer Widerstand of 9.62E-7 Ω·m

400.0 °C

1.01E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.01E-6 Ω·m

500.0 °C

1.06E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.06E-6 Ω·m

600.0 °C

1.1E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.1E-6 Ω·m

700.0 °C

1.13E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.13E-6 Ω·m

800.0 °C

1.16E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.16E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Chrom

16.5 - 18.5 %

Show Material materials with Chrom of 16.5 - 18.5 %

Kohlenstoff

0.03 %

Show Material materials with Kohlenstoff of 0.03 %

Mangan

2 %

Show Material materials with Mangan of 2 %

Molybdän

2.5 - 3 %

Show Material materials with Molybdän of 2.5 - 3 %

Nickel

11 - 14 %

Show Material materials with Nickel of 11 - 14 %

Phosphor

0.05 %

Show Material materials with Phosphor of 0.05 %

Schwefel

0.015 %

Show Material materials with Schwefel of 0.015 %

Silizium

1 %

Show Material materials with Silizium of 1 %

Stickstoff

0.12 - 0.22 %

Show Material materials with Stickstoff of 0.12 - 0.22 %