Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat |
20 °C | 7.84 - 7.86 g/cm³ Show Material materials with Dichte of 7.84 - 7.86 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 7.86 g/cm³ Show Material materials with Dichte of 7.86 g/cm³ | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 15.0 % Show Material materials with Dehnung of 15.0 % | Predicted Value, A200 | ||||
16.0 % Show Material materials with Dehnung of 16.0 % | Predicted Value, A80 Transverse | |||||
16.4 % Show Material materials with Dehnung of 16.4 % | Predicted Value, A80 | |||||
18.0 % Show Material materials with Dehnung of 18.0 % | Predicted Value, A5 | |||||
20.6 % Show Material materials with Dehnung of 20.6 % | Predicted Value, A50 | |||||
20 °C | 18 % Show Material materials with Dehnung of 18 % | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 18 % Show Material materials with Dehnung of 18 % | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | |
20 °C | 211 GPa Show Material materials with Elastizitätsmodul of 211 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 211 - 212 GPa Show Material materials with Elastizitätsmodul of 211 - 212 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
100 °C | 206 GPa Show Material materials with Elastizitätsmodul of 206 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 206 - 207 GPa Show Material materials with Elastizitätsmodul of 206 - 207 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
300 °C | 191 GPa Show Material materials with Elastizitätsmodul of 191 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 191 - 192 GPa Show Material materials with Elastizitätsmodul of 191 - 192 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
400 °C | 183 GPa Show Material materials with Elastizitätsmodul of 183 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 183 - 184 GPa Show Material materials with Elastizitätsmodul of 183 - 184 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
500 °C | 173 GPa Show Material materials with Elastizitätsmodul of 173 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 173 - 175 GPa Show Material materials with Elastizitätsmodul of 173 - 175 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
Flächenreduzierung | 42.9 % Show Material materials with Flächenreduzierung of 42.9 % | Predicted Value | ||||
43.6 % Show Material materials with Flächenreduzierung of 43.6 % | Predicted Value, Transverse | |||||
Härte, Brinell | 251 [-] Show Material materials with Härte, Brinell of 251 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Nickel Molybdenum Steel | ||||
Scherfestigkeit | 617.4 MPa Show Material materials with Scherfestigkeit of 617.4 MPa | Predicted Value | ||||
Schubmodule | 80.9 GPa Show Material materials with Schubmodule of 80.9 GPa | Predicted Value | ||||
Zugfestigkeit | 20 °C | 560 - 750 MPa Show Material materials with Zugfestigkeit of 560 - 750 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse |
20 °C | 560 - 730 MPa Show Material materials with Zugfestigkeit of 560 - 730 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 560 - 710 MPa Show Material materials with Zugfestigkeit of 560 - 710 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 560 - 700 MPa Show Material materials with Zugfestigkeit of 560 - 700 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 560 - 750 MPa Show Material materials with Zugfestigkeit of 560 - 750 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 560 - 730 MPa Show Material materials with Zugfestigkeit of 560 - 730 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 560 - 710 MPa Show Material materials with Zugfestigkeit of 560 - 710 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 560 - 700 MPa Show Material materials with Zugfestigkeit of 560 - 700 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 570 - 750 MPa Show Material materials with Zugfestigkeit of 570 - 750 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 570 - 730 MPa Show Material materials with Zugfestigkeit of 570 - 730 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 570 - 710 MPa Show Material materials with Zugfestigkeit of 570 - 710 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 570 - 700 MPa Show Material materials with Zugfestigkeit of 570 - 700 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 570 - 750 MPa Show Material materials with Zugfestigkeit of 570 - 750 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 570 - 730 MPa Show Material materials with Zugfestigkeit of 570 - 730 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 570 - 710 MPa Show Material materials with Zugfestigkeit of 570 - 710 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 570 - 700 MPa Show Material materials with Zugfestigkeit of 570 - 700 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 590 - 750 MPa Show Material materials with Zugfestigkeit of 590 - 750 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 590 - 730 MPa Show Material materials with Zugfestigkeit of 590 - 730 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 590 - 710 MPa Show Material materials with Zugfestigkeit of 590 - 710 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 590 - 700 MPa Show Material materials with Zugfestigkeit of 590 - 700 MPa | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet, Flat | Transverse | |
20 °C | 590 - 750 MPa Show Material materials with Zugfestigkeit of 590 - 750 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 590 - 730 MPa Show Material materials with Zugfestigkeit of 590 - 730 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 590 - 710 MPa Show Material materials with Zugfestigkeit of 590 - 710 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 590 - 700 MPa Show Material materials with Zugfestigkeit of 590 - 700 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
100 °C | 1.21e-05 - 1.24e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 - 1.24e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
100 °C | 1.24e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.24e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 - 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 - 1.29e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
200 °C | 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 - 1.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.35e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
300 °C | 1.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.35e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 - 1.39e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 - 1.39e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
400 °C | 1.39e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.39e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 - 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 - 1.44e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
500 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
Max. Betriebstemperatur | 20 - 400 °C Show Material materials with Max. Betriebstemperatur of 20 - 400 °C | quenched and tempered (+QT) | EN 10028-2 | Flat | Long | |
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Nickel Molybdenum Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | |
20 °C | 430 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 - 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 - 500 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
100 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 - 540 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
200 °C | 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 540 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 - 580 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
300 °C | 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 580 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 - 620 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
400 °C | 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 620 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 - 690 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
500 °C | 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 690 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
Temperaturleitfähigkeit | 20 °C | 12.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.2 mm²/s | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | |
100 °C | 11.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.3 mm²/s | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
200 °C | 10.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.3 mm²/s | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
300 °C | 9.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.2 mm²/s | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
400 °C | 8.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.1 mm²/s | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
500 °C | 7 mm²/s Show Material materials with Temperaturleitfähigkeit of 7 mm²/s | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
600 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
Wärmeleitfähigkeit | 20 °C | 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 42 - 44.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 - 44.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 44.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 44.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
100 °C | 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 43 - 44 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43 - 44 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 44 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 44 W/(m·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
200 °C | 42.9 - 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42.9 - 43 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 42.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42.9 W/(m·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
200 °C | 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 40.8 - 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.8 - 41 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 40.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.8 W/(m·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
300 °C | 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 38.4 - 39 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.4 - 39 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 38.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.4 W/(m·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
400 °C | 39 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 36 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 36 - 36.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 - 36.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 36.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
600 °C | 33.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33.9 W/(m·K) | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 7 S/m Show Material materials with Elektrische Leitfähigkeit of 7 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 2.35e-07 - 2.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.35e-07 - 2.5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 2.35e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.35e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
20 °C | 2.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 2.91e-07 - 3e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.91e-07 - 3e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 2.91e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.91e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
100 °C | 3e-07 Ω·m Show Material materials with spezifischer Widerstand of 3e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.68e-07 - 3.7e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.68e-07 - 3.7e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.68e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.68e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
200 °C | 3.7e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.7e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.6e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.6e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
400 °C | 5.6e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.6e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.6e-07 - 5.66e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.6e-07 - 5.66e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.66e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.66e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
500 °C | 6.8e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.8e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.8e-07 - 6.81e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.8e-07 - 6.81e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.81e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.81e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet | ||
600 °C | 8.18e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.18e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.01 - 0.05 % Show Material materials with Aluminium of 0.01 - 0.05 % | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet |
Chrom | 0.2 % Show Material materials with Chrom of 0.2 % | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet |
Kohlenstoff | 0.15 - 0.23 % Show Material materials with Kohlenstoff of 0.15 - 0.23 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
0.23 % Show Material materials with Kohlenstoff of 0.23 % | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet | |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Mangan | 1 - 1.5 % Show Material materials with Mangan of 1 - 1.5 % | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet |
Molybdän | 0.4 - 0.6 % Show Material materials with Molybdän of 0.4 - 0.6 % | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet |
0.45 - 0.6 % Show Material materials with Molybdän of 0.45 - 0.6 % | quenched and tempered (+QT) | EN 10028-2 | Flat | |
Nickel | 0.4 - 0.8 % Show Material materials with Nickel of 0.4 - 0.8 % | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
0.015 % Show Material materials with Schwefel of 0.015 % | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet | |
Silizium | 0.15 - 0.35 % Show Material materials with Silizium of 0.15 - 0.35 % | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet |
0.4 % Show Material materials with Silizium of 0.4 % | quenched and tempered (+QT) | EN 10028-2 | Flat | |
Stickstoff | 0.012 % Show Material materials with Stickstoff of 0.012 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
0.015 % Show Material materials with Stickstoff of 0.015 % | quenched and tempered (+QT) | SEW 028, EN 10028-2 | Sheet | |
Vanadium | 0.02 % Show Material materials with Vanadium of 0.02 % | quenched and tempered (+QT) | EN 10028-2, SEW 028 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |