Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.56 - 7.7 g/cm³ Show Material materials with Dichte of 7.56 - 7.7 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 20.0 °C | 218 - 220 GPa Show Material materials with Elastizitätsmodul of 218 - 220 GPa | |
100.0 °C | 213 - 218 GPa Show Material materials with Elastizitätsmodul of 213 - 218 GPa | ||
200.0 °C | 206 - 212 GPa Show Material materials with Elastizitätsmodul of 206 - 212 GPa | ||
300.0 °C | 198 - 205 GPa Show Material materials with Elastizitätsmodul of 198 - 205 GPa | ||
400.0 °C | 190 - 197 GPa Show Material materials with Elastizitätsmodul of 190 - 197 GPa | ||
500.0 °C | 180 GPa Show Material materials with Elastizitätsmodul of 180 GPa | ||
600.0 °C | 167 GPa Show Material materials with Elastizitätsmodul of 167 GPa | ||
700.0 °C | 150 GPa Show Material materials with Elastizitätsmodul of 150 GPa | ||
Härte, Brinell | 20.0 °C | 280 [-] Show Material materials with Härte, Brinell of 280 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Martensitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Martensitic Stainless Steel |
Zugfestigkeit | 20.0 °C | 900 MPa Show Material materials with Zugfestigkeit of 900 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20.0 °C | 9.9E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.9E-6 1/K | |
100.0 °C | 1.03E-5 - 1.05E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.03E-5 - 1.05E-5 1/K | ||
200.0 °C | 1.08E-5 - 1.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08E-5 - 1.1E-5 1/K | ||
300.0 °C | 1.1E-5 - 1.12E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 - 1.12E-5 1/K | ||
400.0 °C | 1.15E-5 - 1.16E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15E-5 - 1.16E-5 1/K | ||
500.0 °C | 1.19E-5 - 1.2E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19E-5 - 1.2E-5 1/K | ||
600.0 °C | 1.21E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.24E-5 1/K | ||
800.0 °C | 1.29E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29E-5 1/K | ||
Schmelzpunkt | 1370 - 1530 °C Show Material materials with Schmelzpunkt of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 450 - 460 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 450 - 460 J/(kg·K) | |
100.0 °C | 482 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 482 J/(kg·K) | ||
200.0 °C | 506 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 506 J/(kg·K) | ||
300.0 °C | 525 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 525 J/(kg·K) | ||
400.0 °C | 547 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 547 J/(kg·K) | ||
500.0 °C | 576 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 576 J/(kg·K) | ||
600.0 °C | 616 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 616 J/(kg·K) | ||
Temperaturleitfähigkeit | 20.0 °C | 4.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.7 mm²/s | |
100.0 °C | 4.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.5 mm²/s | ||
200.0 °C | 4.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.5 mm²/s | ||
300.0 °C | 4.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.6 mm²/s | ||
400.0 °C | 4.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.4 mm²/s | ||
500.0 °C | 4.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.1 mm²/s | ||
600.0 °C | 3.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 3.6 mm²/s | ||
Wärmeleitfähigkeit | 20.0 °C | 16 - 30 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 16 - 30 W/(m·K) | |
100.0 °C | 17.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 17.2 W/(m·K) | ||
200.0 °C | 18.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 18.6 W/(m·K) | ||
300.0 °C | 20 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 20 W/(m·K) | ||
400.0 °C | 21.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 21.2 W/(m·K) | ||
500.0 °C | 22.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 22.3 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 23.3 W/(m·K) | ||
700.0 °C | 24.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 24.1 W/(m·K) | ||
800.0 °C | 25.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25.5 W/(m·K) | ||
900.0 °C | 26.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 26.9 W/(m·K) | ||
1000.0 °C | 28.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 28.3 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 6.5E-7 - 9.06E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.5E-7 - 9.06E-7 Ω·m |
100.0 °C | 9.42E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.42E-7 Ω·m | |
200.0 °C | 9.87E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.87E-7 Ω·m | |
300.0 °C | 1.03E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.03E-6 Ω·m | |
400.0 °C | 1.08E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.08E-6 Ω·m | |
500.0 °C | 1.12E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.12E-6 Ω·m | |
600.0 °C | 1.18E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.18E-6 Ω·m | |
700.0 °C | 1.22E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.22E-6 Ω·m | |
800.0 °C | 1.24E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.24E-6 Ω·m | |
900.0 °C | 1.26E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.26E-6 Ω·m | |
1000.0 °C | 1.27E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.27E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Chrom | 13.8 - 15.8 % Show Material materials with Chrom of 13.8 - 15.8 % |
Kohlenstoff | 0.42 - 0.5 % Show Material materials with Kohlenstoff of 0.42 - 0.5 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Molybdän | 0.45 - 0.6 % Show Material materials with Molybdän of 0.45 - 0.6 % |
Phosphor | 0.05 % Show Material materials with Phosphor of 0.05 % |
Schwefel | 0.03 % Show Material materials with Schwefel of 0.03 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Vanadium | 0.1 - 0.15 % Show Material materials with Vanadium of 0.1 - 0.15 % |