Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.01 g/cm³ Show Material materials with Dichte of 8.01 g/cm³ |
50.0 °C | 8 g/cm³ Show Material materials with Dichte of 8 g/cm³ | |
100.0 °C | 7.98 g/cm³ Show Material materials with Dichte of 7.98 g/cm³ | |
150.0 °C | 7.96 g/cm³ Show Material materials with Dichte of 7.96 g/cm³ | |
200.0 °C | 7.94 g/cm³ Show Material materials with Dichte of 7.94 g/cm³ | |
250.0 °C | 7.91 g/cm³ Show Material materials with Dichte of 7.91 g/cm³ | |
300.0 °C | 7.89 g/cm³ Show Material materials with Dichte of 7.89 g/cm³ | |
350.0 °C | 7.87 g/cm³ Show Material materials with Dichte of 7.87 g/cm³ | |
400.0 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | |
450.0 °C | 7.82 g/cm³ Show Material materials with Dichte of 7.82 g/cm³ | |
500.0 °C | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | |
550.0 °C | 7.77 g/cm³ Show Material materials with Dichte of 7.77 g/cm³ | |
600.0 °C | 7.75 g/cm³ Show Material materials with Dichte of 7.75 g/cm³ | |
650.0 °C | 7.72 g/cm³ Show Material materials with Dichte of 7.72 g/cm³ | |
700.0 °C | 7.7 g/cm³ Show Material materials with Dichte of 7.7 g/cm³ | |
750.0 °C | 7.67 g/cm³ Show Material materials with Dichte of 7.67 g/cm³ | |
800.0 °C | 7.65 g/cm³ Show Material materials with Dichte of 7.65 g/cm³ | |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 22 - 35 % Show Material materials with Dehnung of 22 - 35 % |
Elastizitätsmodul | -100.0 °C | 206 GPa Show Material materials with Elastizitätsmodul of 206 GPa |
20.0 °C | 196 - 198 GPa Show Material materials with Elastizitätsmodul of 196 - 198 GPa | |
50.0 °C | 195.12 GPa Show Material materials with Elastizitätsmodul of 195.12 GPa | |
100.0 °C | 190 - 192 GPa Show Material materials with Elastizitätsmodul of 190 - 192 GPa | |
150.0 °C | 186.88 GPa Show Material materials with Elastizitätsmodul of 186.88 GPa | |
200.0 °C | 182 - 183 GPa Show Material materials with Elastizitätsmodul of 182 - 183 GPa | |
250.0 °C | 178.54 GPa Show Material materials with Elastizitätsmodul of 178.54 GPa | |
300.0 °C | 174 - 175 GPa Show Material materials with Elastizitätsmodul of 174 - 175 GPa | |
350.0 °C | 169.91 GPa Show Material materials with Elastizitätsmodul of 169.91 GPa | |
400.0 °C | 165.69 - 167 GPa Show Material materials with Elastizitätsmodul of 165.69 - 167 GPa | |
450.0 °C | 161.67 GPa Show Material materials with Elastizitätsmodul of 161.67 GPa | |
500.0 °C | 157.55 - 159 GPa Show Material materials with Elastizitätsmodul of 157.55 - 159 GPa | |
550.0 °C | 153.62 GPa Show Material materials with Elastizitätsmodul of 153.62 GPa | |
600.0 °C | 149.8 - 150 GPa Show Material materials with Elastizitätsmodul of 149.8 - 150 GPa | |
650.0 °C | 145.97 GPa Show Material materials with Elastizitätsmodul of 145.97 GPa | |
700.0 °C | 142 - 142.34 GPa Show Material materials with Elastizitätsmodul of 142 - 142.34 GPa | |
750.0 °C | 138.81 GPa Show Material materials with Elastizitätsmodul of 138.81 GPa | |
800.0 °C | 134 - 135.28 GPa Show Material materials with Elastizitätsmodul of 134 - 135.28 GPa | |
Poissonzahl | 20.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] |
50.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
100.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
150.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
250.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
300.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
350.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
400.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
450.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
550.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
600.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
650.0 °C | 0.32 [-] Show Material materials with Poissonzahl of 0.32 [-] | |
700.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | |
750.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | |
800.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | |
Schubmodule | 20.0 °C | 77.3 GPa Show Material materials with Schubmodule of 77.3 GPa |
50.0 °C | 76.32 GPa Show Material materials with Schubmodule of 76.32 GPa | |
100.0 °C | 74.65 GPa Show Material materials with Schubmodule of 74.65 GPa | |
150.0 °C | 72.79 GPa Show Material materials with Schubmodule of 72.79 GPa | |
200.0 °C | 70.83 GPa Show Material materials with Schubmodule of 70.83 GPa | |
250.0 °C | 68.87 GPa Show Material materials with Schubmodule of 68.87 GPa | |
300.0 °C | 67 GPa Show Material materials with Schubmodule of 67 GPa | |
350.0 °C | 65.24 GPa Show Material materials with Schubmodule of 65.24 GPa | |
400.0 °C | 63.47 GPa Show Material materials with Schubmodule of 63.47 GPa | |
450.0 °C | 61.8 GPa Show Material materials with Schubmodule of 61.8 GPa | |
500.0 °C | 60.14 GPa Show Material materials with Schubmodule of 60.14 GPa | |
550.0 °C | 58.57 GPa Show Material materials with Schubmodule of 58.57 GPa | |
600.0 °C | 57 GPa Show Material materials with Schubmodule of 57 GPa | |
650.0 °C | 55.43 GPa Show Material materials with Schubmodule of 55.43 GPa | |
700.0 °C | 53.46 GPa Show Material materials with Schubmodule of 53.46 GPa | |
750.0 °C | 52.39 GPa Show Material materials with Schubmodule of 52.39 GPa | |
800.0 °C | 50.91 GPa Show Material materials with Schubmodule of 50.91 GPa | |
Streckgrenze Rp 0,2 | 20.0 °C | 215 MPa Show Material materials with Streckgrenze Rp 0,2 of 215 MPa |
100.0 °C | 195 MPa Show Material materials with Streckgrenze Rp 0,2 of 195 MPa | |
200.0 °C | 177 MPa Show Material materials with Streckgrenze Rp 0,2 of 177 MPa | |
300.0 °C | 157 MPa Show Material materials with Streckgrenze Rp 0,2 of 157 MPa | |
400.0 °C | 147 MPa Show Material materials with Streckgrenze Rp 0,2 of 147 MPa | |
500.0 °C | 137 MPa Show Material materials with Streckgrenze Rp 0,2 of 137 MPa | |
550.0 °C | 137 MPa Show Material materials with Streckgrenze Rp 0,2 of 137 MPa | |
600.0 °C | 132 MPa Show Material materials with Streckgrenze Rp 0,2 of 132 MPa | |
Streckgrenze Rp 1,0 | 20.0 °C | 255 MPa Show Material materials with Streckgrenze Rp 1,0 of 255 MPa |
100.0 °C | 225 MPa Show Material materials with Streckgrenze Rp 1,0 of 225 MPa | |
200.0 °C | 206 MPa Show Material materials with Streckgrenze Rp 1,0 of 206 MPa | |
300.0 °C | 186 MPa Show Material materials with Streckgrenze Rp 1,0 of 186 MPa | |
400.0 °C | 177 MPa Show Material materials with Streckgrenze Rp 1,0 of 177 MPa | |
500.0 °C | 167 MPa Show Material materials with Streckgrenze Rp 1,0 of 167 MPa | |
550.0 °C | 167 MPa Show Material materials with Streckgrenze Rp 1,0 of 167 MPa | |
600.0 °C | 162 MPa Show Material materials with Streckgrenze Rp 1,0 of 162 MPa | |
Zugfestigkeit | 20.0 °C | 530 - 690 MPa Show Material materials with Zugfestigkeit of 530 - 690 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100.0 °C | 1.49E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.61E-5 1/K | ||
100.0 °C | 1.63E-5 - 1.67E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.63E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.69E-5 - 1.72E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.69E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.73E-5 - 1.77E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.73E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.78E-5 - 1.81E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.78E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.82E-5 - 1.84E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.82E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.85E-5 - 1.88E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.85E-5 - 1.88E-5 1/K | ||
700.0 °C | 1.87E-5 - 1.91E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.87E-5 - 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2E-5 1/K | ||
Max. Betriebstemperatur, lang | 0 - 700 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 700 °C | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | -100.0 °C | 440 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 440 J/(kg·K) | |
20.0 °C | 450 - 472 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 450 - 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 571 J/(kg·K) | ||
Temperaturleitfähigkeit | 20.0 °C | 3.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 3.6 mm²/s | |
100.0 °C | 3.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 3.7 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Temperaturleitfähigkeit of 4 mm²/s | ||
300.0 °C | 4.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.4 mm²/s | ||
400.0 °C | 4.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.6 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.7 mm²/s | ||
600.0 °C | 4.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.9 mm²/s | ||
700.0 °C | 5.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.2 mm²/s | ||
800.0 °C | 5.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.5 mm²/s | ||
Wärmeleitfähigkeit | 20.0 °C | 13.5 - 16 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 13.5 - 16 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 14.9 W/(m·K) | ||
200.0 °C | 16.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 16.7 W/(m·K) | ||
300.0 °C | 18.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 18.3 W/(m·K) | ||
400.0 °C | 19.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 19.8 W/(m·K) | ||
500.0 °C | 21.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 21.3 W/(m·K) | ||
600.0 °C | 22.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 22.7 W/(m·K) | ||
700.0 °C | 24.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 24.2 W/(m·K) | ||
800.0 °C | 25.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25.6 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 7.75E-7 - 8.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.75E-7 - 8.5E-7 Ω·m |
50.0 °C | 8E-7 Ω·m Show Material materials with spezifischer Widerstand of 8E-7 Ω·m | |
100.0 °C | 8.42E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.42E-7 Ω·m | |
150.0 °C | 8.74E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.74E-7 Ω·m | |
200.0 °C | 9.04E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.04E-7 Ω·m | |
250.0 °C | 9.35E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.35E-7 Ω·m | |
300.0 °C | 9.62E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.62E-7 Ω·m | |
350.0 °C | 9.9E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.9E-7 Ω·m | |
400.0 °C | 1.01E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.01E-6 Ω·m | |
450.0 °C | 1.04E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.04E-6 Ω·m | |
500.0 °C | 1.06E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.06E-6 Ω·m | |
550.0 °C | 1.08E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.08E-6 Ω·m | |
600.0 °C | 1.1E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.1E-6 Ω·m | |
650.0 °C | 1.11E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.11E-6 Ω·m | |
700.0 °C | 1.13E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.13E-6 Ω·m | |
750.0 °C | 1.15E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.15E-6 Ω·m | |
800.0 °C | 1.16E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.16E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Chrom | 15.5 - 17.5 % Show Material materials with Chrom of 15.5 - 17.5 % |
Kohlenstoff | 0.04 - 0.1 % Show Material materials with Kohlenstoff of 0.04 - 0.1 % |
Mangan | 1.5 % Show Material materials with Mangan of 1.5 % |
Molybdän | 1.6 - 2 % Show Material materials with Molybdän of 1.6 - 2 % |
Nickel | 15.5 - 17.5 % Show Material materials with Nickel of 15.5 - 17.5 % |
Phosphor | 0.04 % Show Material materials with Phosphor of 0.04 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 0.3 - 0.6 % Show Material materials with Silizium of 0.3 - 0.6 % |