Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 26 % Show Material materials with Dehnung of 26 % | |
Dehnung, transversal | 20.0 °C | 24 % Show Material materials with Dehnung, transversal of 24 % | |
Elastizitätsmodul | 23.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel |
Poissonzahl | 23.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel |
Schubmodule | 23.0 °C | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel |
Streckgrenze | 20.0 °C | 225 - 235 MPa Show Material materials with Streckgrenze of 225 - 235 MPa | |
Zugfestigkeit | 20.0 °C | 340 - 470 MPa Show Material materials with Zugfestigkeit of 340 - 470 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.32E-5 - 1.38E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32E-5 - 1.38E-5 1/K | Typical for Low Carbon Steel |
Max. Betriebstemperatur | 500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Spezifische Wärmekapazität | 23.0 °C | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | Typical for Low Carbon Steel |
Wärmeleitfähigkeit | 23.0 °C | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
spezifischer Widerstand | 23.0 °C | 1.43E-7 - 1.74E-7 Ω·m Show Material materials with spezifischer Widerstand of 1.43E-7 - 1.74E-7 Ω·m | Typical for Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |