Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20 °C | 16 % Show Material materials with Dehnung of 16 % | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
Poissonzahl | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel | ||||
Streckgrenze | 20 °C | 410 MPa Show Material materials with Streckgrenze of 410 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
20 °C | 420 MPa Show Material materials with Streckgrenze of 420 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 430 MPa Show Material materials with Streckgrenze of 430 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 440 MPa Show Material materials with Streckgrenze of 440 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 450 MPa Show Material materials with Streckgrenze of 450 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 460 MPa Show Material materials with Streckgrenze of 460 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 470 MPa Show Material materials with Streckgrenze of 470 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 480 MPa Show Material materials with Streckgrenze of 480 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 500 MPa Show Material materials with Streckgrenze of 500 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
Zugfestigkeit | 20 °C | 570 - 780 MPa Show Material materials with Zugfestigkeit of 570 - 780 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
20 °C | 570 - 770 MPa Show Material materials with Zugfestigkeit of 570 - 770 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 570 - 760 MPa Show Material materials with Zugfestigkeit of 570 - 760 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 570 - 750 MPa Show Material materials with Zugfestigkeit of 570 - 750 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 570 - 740 MPa Show Material materials with Zugfestigkeit of 570 - 740 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 580 - 780 MPa Show Material materials with Zugfestigkeit of 580 - 780 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 580 - 770 MPa Show Material materials with Zugfestigkeit of 580 - 770 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 580 - 760 MPa Show Material materials with Zugfestigkeit of 580 - 760 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 580 - 750 MPa Show Material materials with Zugfestigkeit of 580 - 750 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 580 - 740 MPa Show Material materials with Zugfestigkeit of 580 - 740 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 590 - 780 MPa Show Material materials with Zugfestigkeit of 590 - 780 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 590 - 770 MPa Show Material materials with Zugfestigkeit of 590 - 770 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 590 - 760 MPa Show Material materials with Zugfestigkeit of 590 - 760 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 590 - 750 MPa Show Material materials with Zugfestigkeit of 590 - 750 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 590 - 740 MPa Show Material materials with Zugfestigkeit of 590 - 740 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 600 - 780 MPa Show Material materials with Zugfestigkeit of 600 - 780 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 600 - 770 MPa Show Material materials with Zugfestigkeit of 600 - 770 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 600 - 760 MPa Show Material materials with Zugfestigkeit of 600 - 760 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 600 - 750 MPa Show Material materials with Zugfestigkeit of 600 - 750 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 600 - 740 MPa Show Material materials with Zugfestigkeit of 600 - 740 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 610 - 780 MPa Show Material materials with Zugfestigkeit of 610 - 780 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 610 - 770 MPa Show Material materials with Zugfestigkeit of 610 - 770 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 610 - 760 MPa Show Material materials with Zugfestigkeit of 610 - 760 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 610 - 750 MPa Show Material materials with Zugfestigkeit of 610 - 750 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | ||
20 °C | 610 - 740 MPa Show Material materials with Zugfestigkeit of 610 - 740 MPa | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
Temperaturleitfähigkeit | -100 °C | 11.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.9 mm²/s | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
20 °C | 11 mm²/s Show Material materials with Temperaturleitfähigkeit of 11 mm²/s | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
100 °C | 10.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.5 mm²/s | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
200 °C | 9.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.9 mm²/s | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
300 °C | 9.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.1 mm²/s | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
400 °C | 8.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.1 mm²/s | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
500 °C | 6.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.9 mm²/s | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
600 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
Wärmeleitfähigkeit | -100 °C | 34.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.7 W/(m·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
20 °C | 39.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.7 W/(m·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
100 °C | 40.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.9 W/(m·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
200 °C | 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41 W/(m·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
300 °C | 39.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.9 W/(m·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
400 °C | 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.2 W/(m·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
500 °C | 36.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.1 W/(m·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
600 °C | 33.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33.8 W/(m·K) | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
spezifischer Widerstand | -100 °C | 1.97e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.97e-07 Ω·m | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
20 °C | 2.62e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.62e-07 Ω·m | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
100 °C | 3.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.13e-07 Ω·m | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
200 °C | 3.85e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-07 Ω·m | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
300 °C | 4.7e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.7e-07 Ω·m | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
400 °C | 5.69e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.69e-07 Ω·m | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
500 °C | 6.85e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.85e-07 Ω·m | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar | |
600 °C | 8.2e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.2e-07 Ω·m | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Chrom | 0.3 Show Material materials with Chrom of 0.3 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Kohlenstoff | 0.21 Show Material materials with Kohlenstoff of 0.21 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Kupfer | 0.2 Show Material materials with Kupfer of 0.2 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Mangan | 1 - 1.7 % Show Material materials with Mangan of 1 - 1.7 % | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Molybdän | 0.1 Show Material materials with Molybdän of 0.1 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Nickel | 1 Show Material materials with Nickel of 1 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Niobium | 0.05 Show Material materials with Niobium of 0.05 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Phosphor | 0.03 Show Material materials with Phosphor of 0.03 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Schwefel | 0.025 Show Material materials with Schwefel of 0.025 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Silizium | 0.1 - 0.6 % Show Material materials with Silizium of 0.1 - 0.6 % | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Stickstoff | 0.02 Show Material materials with Stickstoff of 0.02 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |
Vanadium | 0.22 Show Material materials with Vanadium of 0.22 | normalized or normalized formed (+N) | DIN 17102, EN 10025-1, EN 10025-3, EN 10028-1, EN 10028-3, DIN 17103 | Sheet, Strip, Bar |