Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.9 g/cm³ Show Material materials with Dichte of 7.9 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 30 % Show Material materials with Dehnung of 30 % | |
Elastizitätsmodul | 23.0 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | Typical for Austenitic Stainless Steel |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 1,0 | 20.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 1,0 of 220 MPa | |
100.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 1,0 of 175 MPa | ||
200.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 1,0 of 145 MPa | ||
300.0 °C | 115 MPa Show Material materials with Streckgrenze Rp 1,0 of 115 MPa | ||
400.0 °C | 105 MPa Show Material materials with Streckgrenze Rp 1,0 of 105 MPa | ||
Zugfestigkeit | 20.0 °C | 440 - 640 MPa Show Material materials with Zugfestigkeit of 440 - 640 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.58E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.58E-5 1/K | |
300.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | ||
500.0 °C | 1.77E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.77E-5 1/K | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 530 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 530 J/(kg·K) | |
Wärmeleitfähigkeit | 50.0 °C | 14.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 14.5 W/(m·K) | |
100.0 °C | 15.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 15.8 W/(m·K) | ||
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
spezifischer Widerstand | 23.0 °C | 8.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Chrom | 18 - 20 % Show Material materials with Chrom of 18 - 20 % |
Kohlenstoff | 0.03 % Show Material materials with Kohlenstoff of 0.03 % |
Mangan | 2 % Show Material materials with Mangan of 2 % |
Molybdän | 2 - 2.5 % Show Material materials with Molybdän of 2 - 2.5 % |
Nickel | 9 - 12 % Show Material materials with Nickel of 9 - 12 % |
Phosphor | 0.04 % Show Material materials with Phosphor of 0.04 % |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % |
Silizium | 1.5 % Show Material materials with Silizium of 1.5 % |
Stickstoff | 0.2 % Show Material materials with Stickstoff of 0.2 % |