Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 15.9 % Show Material materials with Dehnung of 15.9 % | Predicted Value, A80 | ||||
16.4 % Show Material materials with Dehnung of 16.4 % | Predicted Value, A80 Transverse | |||||
18.0 % Show Material materials with Dehnung of 18.0 % | Predicted Value, A200 | |||||
20.5 % Show Material materials with Dehnung of 20.5 % | Predicted Value, A5 | |||||
25.8 % Show Material materials with Dehnung of 25.8 % | Predicted Value, A50 | |||||
20 °C | 17 % Show Material materials with Dehnung of 17 % | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 17 % Show Material materials with Dehnung of 17 % | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 18 % Show Material materials with Dehnung of 18 % | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 212 - 214 GPa Show Material materials with Elastizitätsmodul of 212 - 214 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 212 - 212.4 GPa Show Material materials with Elastizitätsmodul of 212 - 212.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 212.4 - 214 GPa Show Material materials with Elastizitätsmodul of 212.4 - 214 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 212.4 GPa Show Material materials with Elastizitätsmodul of 212.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 214 GPa Show Material materials with Elastizitätsmodul of 214 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207 - 209 GPa Show Material materials with Elastizitätsmodul of 207 - 209 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207 - 207.5 GPa Show Material materials with Elastizitätsmodul of 207 - 207.5 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207.5 - 209 GPa Show Material materials with Elastizitätsmodul of 207.5 - 209 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207.5 GPa Show Material materials with Elastizitätsmodul of 207.5 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 209 GPa Show Material materials with Elastizitätsmodul of 209 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 199 - 202 GPa Show Material materials with Elastizitätsmodul of 199 - 202 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 199 - 201.2 GPa Show Material materials with Elastizitätsmodul of 199 - 201.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 201.2 - 202 GPa Show Material materials with Elastizitätsmodul of 201.2 - 202 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 201.2 GPa Show Material materials with Elastizitätsmodul of 201.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 202 GPa Show Material materials with Elastizitätsmodul of 202 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 192 - 195 GPa Show Material materials with Elastizitätsmodul of 192 - 195 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 192 - 193.9 GPa Show Material materials with Elastizitätsmodul of 192 - 193.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 193.9 - 195 GPa Show Material materials with Elastizitätsmodul of 193.9 - 195 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 193.9 GPa Show Material materials with Elastizitätsmodul of 193.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184 - 187 GPa Show Material materials with Elastizitätsmodul of 184 - 187 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184 - 185.2 GPa Show Material materials with Elastizitätsmodul of 184 - 185.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 185.2 - 187 GPa Show Material materials with Elastizitätsmodul of 185.2 - 187 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 185.2 GPa Show Material materials with Elastizitätsmodul of 185.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 187 GPa Show Material materials with Elastizitätsmodul of 187 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 174.9 - 177 GPa Show Material materials with Elastizitätsmodul of 174.9 - 177 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 174.9 - 175 GPa Show Material materials with Elastizitätsmodul of 174.9 - 175 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 174.9 GPa Show Material materials with Elastizitätsmodul of 174.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 175 - 177 GPa Show Material materials with Elastizitätsmodul of 175 - 177 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 177 GPa Show Material materials with Elastizitätsmodul of 177 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 163.2 - 167 GPa Show Material materials with Elastizitätsmodul of 163.2 - 167 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 163.2 - 164 GPa Show Material materials with Elastizitätsmodul of 163.2 - 164 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 163.2 GPa Show Material materials with Elastizitätsmodul of 163.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 164 - 167 GPa Show Material materials with Elastizitätsmodul of 164 - 167 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 167 GPa Show Material materials with Elastizitätsmodul of 167 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Flächenreduzierung | 42.0 % Show Material materials with Flächenreduzierung of 42.0 % | Predicted Value | ||||
45.5 % Show Material materials with Flächenreduzierung of 45.5 % | Predicted Value, Transverse | |||||
Poissonzahl | 20 °C | 0.283 [-] Show Material materials with Poissonzahl of 0.283 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | |
100 °C | 0.286 [-] Show Material materials with Poissonzahl of 0.286 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 0.292 [-] Show Material materials with Poissonzahl of 0.292 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 0.294 [-] Show Material materials with Poissonzahl of 0.294 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 0.307 [-] Show Material materials with Poissonzahl of 0.307 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 0.313 [-] Show Material materials with Poissonzahl of 0.313 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Scherfestigkeit | 605.2 MPa Show Material materials with Scherfestigkeit of 605.2 MPa | Predicted Value | ||||
Schubmodule | 20 °C | 82.8 GPa Show Material materials with Schubmodule of 82.8 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | |
100 °C | 80.7 GPa Show Material materials with Schubmodule of 80.7 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 77.9 GPa Show Material materials with Schubmodule of 77.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 74.9 GPa Show Material materials with Schubmodule of 74.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 71.2 GPa Show Material materials with Schubmodule of 71.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 66.9 GPa Show Material materials with Schubmodule of 66.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 62.1 GPa Show Material materials with Schubmodule of 62.1 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Streckgrenze | 265.6 MPa Show Material materials with Streckgrenze of 265.6 MPa | Predicted Value, RP1 Transverse | ||||
265.9 MPa Show Material materials with Streckgrenze of 265.9 MPa | Predicted Value, RP1 | |||||
379.2 MPa Show Material materials with Streckgrenze of 379.2 MPa | Predicted Value, RP05 | |||||
382.3 MPa Show Material materials with Streckgrenze of 382.3 MPa | Predicted Value, RP02 Transverse | |||||
485.8 MPa Show Material materials with Streckgrenze of 485.8 MPa | Predicted Value, RP002 | |||||
20 °C | 250 MPa Show Material materials with Streckgrenze of 250 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 250 MPa Show Material materials with Streckgrenze of 250 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 260 MPa Show Material materials with Streckgrenze of 260 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 260 MPa Show Material materials with Streckgrenze of 260 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 290 MPa Show Material materials with Streckgrenze of 290 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
50 °C | 240 MPa Show Material materials with Streckgrenze of 240 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
50 °C | 250 MPa Show Material materials with Streckgrenze of 250 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
100 °C | 227 MPa Show Material materials with Streckgrenze of 227 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
100 °C | 237 MPa Show Material materials with Streckgrenze of 237 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
150 °C | 219 MPa Show Material materials with Streckgrenze of 219 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
150 °C | 228 MPa Show Material materials with Streckgrenze of 228 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
200 °C | 213 MPa Show Material materials with Streckgrenze of 213 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
200 °C | 222 MPa Show Material materials with Streckgrenze of 222 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
250 °C | 210 MPa Show Material materials with Streckgrenze of 210 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
250 °C | 219 MPa Show Material materials with Streckgrenze of 219 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
300 °C | 208 MPa Show Material materials with Streckgrenze of 208 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
300 °C | 213 MPa Show Material materials with Streckgrenze of 213 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
350 °C | 204 MPa Show Material materials with Streckgrenze of 204 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
400 °C | 191 MPa Show Material materials with Streckgrenze of 191 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
450 °C | 178 MPa Show Material materials with Streckgrenze of 178 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
500 °C | 167 MPa Show Material materials with Streckgrenze of 167 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
Zugfestigkeit | 20 °C | 450 - 630 MPa Show Material materials with Zugfestigkeit of 450 - 630 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse |
20 °C | 450 - 610 MPa Show Material materials with Zugfestigkeit of 450 - 610 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit of 450 - 600 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 450 - 610 MPa Show Material materials with Zugfestigkeit of 450 - 610 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit of 450 - 600 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 460 - 630 MPa Show Material materials with Zugfestigkeit of 460 - 630 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 460 - 610 MPa Show Material materials with Zugfestigkeit of 460 - 610 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 460 - 600 MPa Show Material materials with Zugfestigkeit of 460 - 600 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 460 - 610 MPa Show Material materials with Zugfestigkeit of 460 - 610 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 460 - 600 MPa Show Material materials with Zugfestigkeit of 460 - 600 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 480 - 630 MPa Show Material materials with Zugfestigkeit of 480 - 630 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 480 - 610 MPa Show Material materials with Zugfestigkeit of 480 - 610 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 480 - 600 MPa Show Material materials with Zugfestigkeit of 480 - 600 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 - 1.22e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 - 1.22e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 1.22e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.22e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 - 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 - 1.29e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 - 1.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.34e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.34e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 - 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 - 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 - 1.43e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 - 1.43e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.43e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 - 1.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 - 1.46e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.46e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 - 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 - 500 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 - 540 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 540 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 - 580 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 580 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 - 620 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 620 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 - 690 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 690 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 587 - 780 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 - 780 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 780 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 780 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Temperaturleitfähigkeit | 20 °C | 9.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | |
100 °C | 9.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.6 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 9.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.2 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 8.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.5 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 7.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.8 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.8 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Wärmeleitfähigkeit | 20 °C | 34.9 - 35 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.9 - 35 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 34.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.9 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 35 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 37 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 37 - 37.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37 - 37.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 37.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 38 - 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 - 38.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 37.8 - 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.8 - 38 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 37.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.8 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 36.6 - 37 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.6 - 37 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 36.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 37 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 35 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 35 - 35.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35 - 35.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 35.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 33 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 33 - 33.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33 - 33.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 33.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 3 S/m Show Material materials with Elektrische Leitfähigkeit of 3 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 2.98e-07 - 3e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.98e-07 - 3e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 2.98e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.98e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 3e-07 Ω·m Show Material materials with spezifischer Widerstand of 3e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 3.4e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 3.4e-07 - 3.43e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-07 - 3.43e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 3.43e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.43e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 4.1e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 4.1e-07 - 4.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-07 - 4.13e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 4.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.13e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.97e-07 - 5e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.97e-07 - 5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.97e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.97e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 5e-07 Ω·m Show Material materials with spezifischer Widerstand of 5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.9e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.9e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.9e-07 - 5.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.9e-07 - 5.95e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.95e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 7e-07 Ω·m Show Material materials with spezifischer Widerstand of 7e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 7e-07 - 7.03e-07 Ω·m Show Material materials with spezifischer Widerstand of 7e-07 - 7.03e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 7.03e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.03e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 8.2e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.2e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 8.2e-07 - 8.25e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.2e-07 - 8.25e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 8.25e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.25e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 2 - 2.5 % Show Material materials with Chrom of 2 - 2.5 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Kohlenstoff | 0.08 - 0.14 % Show Material materials with Kohlenstoff of 0.08 - 0.14 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Mangan | 0.4 - 0.8 % Show Material materials with Mangan of 0.4 - 0.8 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Molybdän | 0.9 - 1.1 % Show Material materials with Molybdän of 0.9 - 1.1 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Stickstoff | 0.012 % Show Material materials with Stickstoff of 0.012 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |