Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | normalized and tempered (+NT) | EN 10028-4 | Flat |
27 °C | 7.858 g/cm³ Show Material materials with Dichte of 7.858 g/cm³ | normalized and tempered (+NT) | EN 10028-4 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 17.4 % Show Material materials with Dehnung of 17.4 % | Predicted Value, A200 | ||||
19.6 % Show Material materials with Dehnung of 19.6 % | Predicted Value, A80 Transverse | |||||
20.5 % Show Material materials with Dehnung of 20.5 % | Predicted Value, A80 | |||||
20.6 % Show Material materials with Dehnung of 20.6 % | Predicted Value, A50 | |||||
20.9 % Show Material materials with Dehnung of 20.9 % | Predicted Value, Transverse | |||||
22.4 % Show Material materials with Dehnung of 22.4 % | Predicted Value, A5 | |||||
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Elastizitätsmodul | -269 °C | 215.3 GPa Show Material materials with Elastizitätsmodul of 215.3 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | |
-200 °C | 214.6 GPa Show Material materials with Elastizitätsmodul of 214.6 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-150 °C | 212.8 GPa Show Material materials with Elastizitätsmodul of 212.8 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-100 °C | 210.4 - 214 GPa Show Material materials with Elastizitätsmodul of 210.4 - 214 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-100 °C | 210.4 GPa Show Material materials with Elastizitätsmodul of 210.4 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-100 °C | 214 GPa Show Material materials with Elastizitätsmodul of 214 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-50 °C | 207.9 GPa Show Material materials with Elastizitätsmodul of 207.9 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
20 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
27 °C | 203.8 GPa Show Material materials with Elastizitätsmodul of 203.8 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 202 GPa Show Material materials with Elastizitätsmodul of 202 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 196 GPa Show Material materials with Elastizitätsmodul of 196 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 189 GPa Show Material materials with Elastizitätsmodul of 189 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 181 GPa Show Material materials with Elastizitätsmodul of 181 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Flächenreduzierung | 42.8 % Show Material materials with Flächenreduzierung of 42.8 % | Predicted Value, Transverse | ||||
43.0 % Show Material materials with Flächenreduzierung of 43.0 % | Predicted Value | |||||
Poissonzahl | -269 °C | 0.282 [-] Show Material materials with Poissonzahl of 0.282 [-] | normalized and tempered (+NT) | EN 10028-4 | Flat | |
-200 °C | 0.282 [-] Show Material materials with Poissonzahl of 0.282 [-] | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-150 °C | 0.283 [-] Show Material materials with Poissonzahl of 0.283 [-] | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-100 °C | 0.284 [-] Show Material materials with Poissonzahl of 0.284 [-] | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-50 °C | 0.285 [-] Show Material materials with Poissonzahl of 0.285 [-] | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
27 °C | 0.288 [-] Show Material materials with Poissonzahl of 0.288 [-] | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Scherfestigkeit | 517.5 MPa Show Material materials with Scherfestigkeit of 517.5 MPa | Predicted Value | ||||
Schubmodule | -269 °C | 84 GPa Show Material materials with Schubmodule of 84 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | |
-200 °C | 83.7 GPa Show Material materials with Schubmodule of 83.7 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-150 °C | 82.9 GPa Show Material materials with Schubmodule of 82.9 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-100 °C | 81.9 GPa Show Material materials with Schubmodule of 81.9 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
-50 °C | 80.9 GPa Show Material materials with Schubmodule of 80.9 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
27 °C | 79.1 GPa Show Material materials with Schubmodule of 79.1 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Streckgrenze | 249.6 MPa Show Material materials with Streckgrenze of 249.6 MPa | Predicted Value, RP1 | ||||
313.2 MPa Show Material materials with Streckgrenze of 313.2 MPa | Predicted Value, RP1 Transverse | |||||
345.4 MPa Show Material materials with Streckgrenze of 345.4 MPa | Predicted Value, Transverse | |||||
360.3 MPa Show Material materials with Streckgrenze of 360.3 MPa | Predicted Value, RP05 | |||||
392 MPa Show Material materials with Streckgrenze of 392 MPa | Predicted Value, RP02 | |||||
442.3 MPa Show Material materials with Streckgrenze of 442.3 MPa | Predicted Value, RP02 Transverse | |||||
476.7 MPa Show Material materials with Streckgrenze of 476.7 MPa | Predicted Value, RP002 | |||||
20 °C | 335 MPa Show Material materials with Streckgrenze of 335 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
20 °C | 345 MPa Show Material materials with Streckgrenze of 345 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
20 °C | 355 MPa Show Material materials with Streckgrenze of 355 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Zugfestigkeit | 20 °C | 490 - 640 MPa Show Material materials with Zugfestigkeit of 490 - 640 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.02e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.02e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 1.13e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.13e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 1.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.18e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 1.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.23e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 1.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.31e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Schmelzpunkt | 1316 - 1595 °C Show Material materials with Schmelzpunkt of 1316 - 1595 °C | Typical for Nickel Steel | ||||
Spezifische Wärmekapazität | -100 °C | 441 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 441 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 464 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 464 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 496 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 496 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 513 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 513 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 532 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 532 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Temperaturleitfähigkeit | 20 °C | 9.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.8 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | |
100 °C | 9.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.9 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 9.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.5 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 8.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.7 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 7.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.8 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Wärmeleitfähigkeit | -100 °C | 28.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 28.9 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 35.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.8 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 38.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.1 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 38.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.9 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 36.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.8 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 7 S/m Show Material materials with Elektrische Leitfähigkeit of 7 S/m | Predicted Value | ||||
spezifischer Widerstand | -100 °C | 2e-07 Ω·m Show Material materials with spezifischer Widerstand of 2e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 2.65e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.65e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 3.14e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.14e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 3.79e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.79e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 4.61e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.61e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 5.51e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.51e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Kohlenstoff | 0.15 % Show Material materials with Kohlenstoff of 0.15 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Mangan | 0.3 - 0.8 % Show Material materials with Mangan of 0.3 - 0.8 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Nickel | 3.25 - 3.75 % Show Material materials with Nickel of 3.25 - 3.75 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Schwefel | 0.005 % Show Material materials with Schwefel of 0.005 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
0.01 % Show Material materials with Schwefel of 0.01 % | normalized and tempered (+NT) | EN 10028-4 | Flat | |
Silizium | 0.35 % Show Material materials with Silizium of 0.35 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |