Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.88 g/cm³ Show Material materials with Dichte of 7.88 g/cm³ | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
27 °C | 7.841 g/cm³ Show Material materials with Dichte of 7.841 g/cm³ | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dehnung | 20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Elastizitätsmodul | -269 °C | 205.5 GPa Show Material materials with Elastizitätsmodul of 205.5 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
-200 °C | 205.2 GPa Show Material materials with Elastizitätsmodul of 205.2 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-150 °C | 203.4 GPa Show Material materials with Elastizitätsmodul of 203.4 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-100 °C | 201 GPa Show Material materials with Elastizitätsmodul of 201 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-100 °C | 201 - 201.4 GPa Show Material materials with Elastizitätsmodul of 201 - 201.4 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-100 °C | 201.4 GPa Show Material materials with Elastizitätsmodul of 201.4 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-50 °C | 198.9 GPa Show Material materials with Elastizitätsmodul of 198.9 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
20 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
27 °C | 195.1 GPa Show Material materials with Elastizitätsmodul of 195.1 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
100 °C | 190 GPa Show Material materials with Elastizitätsmodul of 190 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
200 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
300 °C | 178 GPa Show Material materials with Elastizitätsmodul of 178 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
400 °C | 170 GPa Show Material materials with Elastizitätsmodul of 170 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
Poissonzahl | -269 °C | 0.285 [-] Show Material materials with Poissonzahl of 0.285 [-] | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
-200 °C | 0.286 [-] Show Material materials with Poissonzahl of 0.286 [-] | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-150 °C | 0.287 [-] Show Material materials with Poissonzahl of 0.287 [-] | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-100 °C | 0.288 [-] Show Material materials with Poissonzahl of 0.288 [-] | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-50 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
27 °C | 0.292 [-] Show Material materials with Poissonzahl of 0.292 [-] | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
Schubmodule | -269 °C | 80 GPa Show Material materials with Schubmodule of 80 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
-200 °C | 79.8 GPa Show Material materials with Schubmodule of 79.8 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-150 °C | 79 GPa Show Material materials with Schubmodule of 79 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-100 °C | 78.2 GPa Show Material materials with Schubmodule of 78.2 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
-50 °C | 77.1 GPa Show Material materials with Schubmodule of 77.1 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
27 °C | 75.4 GPa Show Material materials with Schubmodule of 75.4 GPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
Streckgrenze | 20 °C | 480 MPa Show Material materials with Streckgrenze of 480 MPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
20 °C | 490 MPa Show Material materials with Streckgrenze of 490 MPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
Zugfestigkeit | 20 °C | 640 - 840 MPa Show Material materials with Zugfestigkeit of 640 - 840 MPa | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.02e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.02e-05 1/K | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
20 °C | 1.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1e-05 1/K | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
100 °C | 1.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.14e-05 1/K | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
200 °C | 1.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.18e-05 1/K | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
300 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
400 °C | 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
Max. Betriebstemperatur | -200 °C Show Material materials with Max. Betriebstemperatur of -200 °C | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | Long | |
-196 °C Show Material materials with Max. Betriebstemperatur of -196 °C | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | Long | ||
Schmelzpunkt | 1316 - 1595 °C Show Material materials with Schmelzpunkt of 1316 - 1595 °C | Typical for Nickel Steel | ||||
Spezifische Wärmekapazität | -100 °C | 442 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 442 J/(kg·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
20 °C | 464 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 464 J/(kg·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
200 °C | 495 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 495 J/(kg·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
300 °C | 511 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 511 J/(kg·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
400 °C | 528 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 528 J/(kg·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
Temperaturleitfähigkeit | 20 °C | 8.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.3 mm²/s | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
100 °C | 8.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.5 mm²/s | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
200 °C | 8.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.4 mm²/s | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
300 °C | 8 mm²/s Show Material materials with Temperaturleitfähigkeit of 8 mm²/s | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
400 °C | 7.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.3 mm²/s | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
Wärmeleitfähigkeit | -100 °C | 23.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 23.9 W/(m·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
20 °C | 30.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 30.2 W/(m·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
100 °C | 32.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 32.8 W/(m·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
200 °C | 34.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.4 W/(m·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
300 °C | 34.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.7 W/(m·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | ||
400 °C | 34 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34 W/(m·K) | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
spezifischer Widerstand | -100 °C | 2.51e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.51e-07 Ω·m | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
20 °C | 3.22e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.22e-07 Ω·m | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
100 °C | 3.73e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.73e-07 Ω·m | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
200 °C | 4.4e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.4e-07 Ω·m | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
300 °C | 5.19e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.19e-07 Ω·m | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
400 °C | 6.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.13e-07 Ω·m | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Kohlenstoff | 0.1 % Show Material materials with Kohlenstoff of 0.1 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Mangan | 0.3 - 0.8 % Show Material materials with Mangan of 0.3 - 0.8 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Molybdän | 0.1 % Show Material materials with Molybdän of 0.1 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Nickel | 8.5 - 10 % Show Material materials with Nickel of 8.5 - 10 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Schwefel | 0.005 % Show Material materials with Schwefel of 0.005 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
0.01 % Show Material materials with Schwefel of 0.01 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat | |
Silizium | 0.35 % Show Material materials with Silizium of 0.35 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | normalized, normalized and tempered (+N+NT) | EN 10028-4 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |