Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
20 °C | 7.8 - 7.85 g/cm³ Show Material materials with Dichte of 7.8 - 7.85 g/cm³ | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
20 °C | 210 - 212 GPa Show Material materials with Elastizitätsmodul of 210 - 212 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
20 °C | 210 GPa Show Material materials with Elastizitätsmodul of 210 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 205 - 207 GPa Show Material materials with Elastizitätsmodul of 205 - 207 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 205 GPa Show Material materials with Elastizitätsmodul of 205 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 195 - 199 GPa Show Material materials with Elastizitätsmodul of 195 - 199 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 185 - 192 GPa Show Material materials with Elastizitätsmodul of 185 - 192 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 185 GPa Show Material materials with Elastizitätsmodul of 185 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 175 - 184 GPa Show Material materials with Elastizitätsmodul of 175 - 184 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
Härte, Brinell | 251 [-] Show Material materials with Härte, Brinell of 251 [-] | Predicted Value, Transverse | ||||
20 °C | 207 [-] Show Material materials with Härte, Brinell of 207 [-] | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Strip, Sheet, Flat, Bar, Wire, Forging | ||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Medium Carbon Steel | ||||
Schubmodule | 20 °C | 81 GPa Show Material materials with Schubmodule of 81 GPa | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.08e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
20 °C | 1.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 1.11e-05 - 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.11e-05 - 1.25e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 1.11e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.11e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 1.21e-05 - 1.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 - 1.3e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 1.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 1.29e-05 - 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29e-05 - 1.36e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 1.35e-05 - 1.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.35e-05 - 1.41e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 1.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.35e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 1.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.41e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
500 °C | 1.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.45e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
600 °C | 1.49e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49e-05 1/K | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
Max. Betriebstemperatur | -25 - 480 °C Show Material materials with Max. Betriebstemperatur of -25 - 480 °C | soft annealed (+A) | EN 10083-1, EN 10083-2, EN 10083-3 | Strip, Sheet, Flat, Bar, Wire, Forging | Long | |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |||||
Schmelzpunkt | 1380 - 1514 °C Show Material materials with Schmelzpunkt of 1380 - 1514 °C | Typical for Medium Carbon Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
20 °C | 461 - 480 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 - 480 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
20 °C | 480 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 480 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 - 500 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 499 - 550 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 - 550 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 550 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 550 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 517 - 590 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 - 590 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 590 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 590 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
Temperaturleitfähigkeit | 20 °C | 11.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.6 mm²/s | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
100 °C | 11.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.3 mm²/s | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 10.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.5 mm²/s | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 9.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.5 mm²/s | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 8.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.3 mm²/s | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
500 °C | 7.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.1 mm²/s | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
600 °C | 5.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.8 mm²/s | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
Wärmeleitfähigkeit | 20 °C | 41.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.7 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
20 °C | 41.7 - 52 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.7 - 52 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
20 °C | 52 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 52 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 43.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.4 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 43.4 - 50.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.4 - 50.6 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
100 °C | 50.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 50.6 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 43.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.2 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 43.2 - 48.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.2 - 48.1 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
200 °C | 48.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 48.1 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 41.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.4 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 41.4 - 45.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.4 - 45.7 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
300 °C | 45.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.7 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
400 °C | 39.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.1 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
500 °C | 36.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.7 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | ||
600 °C | 34.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.1 W/(m·K) | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
spezifischer Widerstand | 20 °C | 1.2e-07 - 2.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.2e-07 - 2.5e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
20 °C | 1.2e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.2e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
20 °C | 2.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.5e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
100 °C | 2.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.95e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
200 °C | 3.65e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.65e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
300 °C | 4.53e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.53e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
400 °C | 5.56e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.56e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
500 °C | 6.74e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.74e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
600 °C | 8.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.13e-07 Ω·m | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.4 % Show Material materials with Chrom of 0.4 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
Kohlenstoff | 0.42 - 0.5 % Show Material materials with Kohlenstoff of 0.42 - 0.5 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, wire, Flat, Sheet, Strip, Forging, Wire |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
Mangan | 0.5 - 0.8 % Show Material materials with Mangan of 0.5 - 0.8 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, wire, Flat, Sheet, Strip, Forging, Wire |
Molybdän | 0.1 % Show Material materials with Molybdän of 0.1 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
Nickel | 0.4 % Show Material materials with Nickel of 0.4 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
0.03 % Show Material materials with Phosphor of 0.03 % | soft annealed (+A) | EN 10083-1, EN 10083-2, ISO 683-1 | Bar, wire, Flat, Sheet, Strip, Forging | |
0.035 % Show Material materials with Phosphor of 0.035 % | soft annealed (+A) | EN 10083-1, EN 10083-2, EN 10083-3, ISO 683-1 | Strip, Sheet, Flat, Bar, Wire, Forging | |
Schwefel | 0.035 % Show Material materials with Schwefel of 0.035 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, wire, Flat, Sheet, Strip, Forging, Wire |
Silizium | 0.1 - 0.4 % Show Material materials with Silizium of 0.1 - 0.4 % | soft annealed (+A) | ISO 683-1, EN 10083-2, EN 10083-1 | Bar, wire, Flat, Sheet, Strip, Forging |
0.4 % Show Material materials with Silizium of 0.4 % | soft annealed (+A) | EN 10083-1, EN 10083-2, ISO 683-1, EN 10083-3 | Bar, wire, Flat, Sheet, Strip, Forging, Wire |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |