Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.85 - 7.86 g/cm³ Show Material materials with Dichte of 7.85 - 7.86 g/cm³ |
50.0 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | |
100.0 °C | 7.82 g/cm³ Show Material materials with Dichte of 7.82 g/cm³ | |
150.0 °C | 7.81 g/cm³ Show Material materials with Dichte of 7.81 g/cm³ | |
200.0 °C | 7.79 g/cm³ Show Material materials with Dichte of 7.79 g/cm³ | |
250.0 °C | 7.77 g/cm³ Show Material materials with Dichte of 7.77 g/cm³ | |
300.0 °C | 7.76 g/cm³ Show Material materials with Dichte of 7.76 g/cm³ | |
350.0 °C | 7.74 g/cm³ Show Material materials with Dichte of 7.74 g/cm³ | |
400.0 °C | 7.72 g/cm³ Show Material materials with Dichte of 7.72 g/cm³ | |
450.0 °C | 7.7 g/cm³ Show Material materials with Dichte of 7.7 g/cm³ | |
500.0 °C | 7.68 g/cm³ Show Material materials with Dichte of 7.68 g/cm³ | |
550.0 °C | 7.66 g/cm³ Show Material materials with Dichte of 7.66 g/cm³ | |
600.0 °C | 7.64 g/cm³ Show Material materials with Dichte of 7.64 g/cm³ | |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 22 % Show Material materials with Dehnung of 22 % |
Dehnung, transversal | 20.0 °C | 20 % Show Material materials with Dehnung, transversal of 20 % |
Elastizitätsmodul | -100.0 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa |
20.0 °C | 212 - 212.48 GPa Show Material materials with Elastizitätsmodul of 212 - 212.48 GPa | |
50.0 °C | 211.6 GPa Show Material materials with Elastizitätsmodul of 211.6 GPa | |
100.0 °C | 207 - 209.25 GPa Show Material materials with Elastizitätsmodul of 207 - 209.25 GPa | |
150.0 °C | 206.11 GPa Show Material materials with Elastizitätsmodul of 206.11 GPa | |
200.0 °C | 199 - 202.48 GPa Show Material materials with Elastizitätsmodul of 199 - 202.48 GPa | |
250.0 °C | 198.36 GPa Show Material materials with Elastizitätsmodul of 198.36 GPa | |
300.0 °C | 192 - 194.14 GPa Show Material materials with Elastizitätsmodul of 192 - 194.14 GPa | |
350.0 °C | 189.82 GPa Show Material materials with Elastizitätsmodul of 189.82 GPa | |
400.0 °C | 184 - 185.51 GPa Show Material materials with Elastizitätsmodul of 184 - 185.51 GPa | |
450.0 °C | 180.99 GPa Show Material materials with Elastizitätsmodul of 180.99 GPa | |
500.0 °C | 175 - 176.48 GPa Show Material materials with Elastizitätsmodul of 175 - 176.48 GPa | |
550.0 °C | 171.97 GPa Show Material materials with Elastizitätsmodul of 171.97 GPa | |
600.0 °C | 164 - 166.97 GPa Show Material materials with Elastizitätsmodul of 164 - 166.97 GPa | |
Poissonzahl | 20.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] |
50.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
100.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
150.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
250.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
300.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
350.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
450.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
500.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
550.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
600.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
Schubmodule | 20.0 °C | 82.6 GPa Show Material materials with Schubmodule of 82.6 GPa |
50.0 °C | 82.21 GPa Show Material materials with Schubmodule of 82.21 GPa | |
100.0 °C | 81.23 GPa Show Material materials with Schubmodule of 81.23 GPa | |
150.0 °C | 79.95 GPa Show Material materials with Schubmodule of 79.95 GPa | |
200.0 °C | 78.48 GPa Show Material materials with Schubmodule of 78.48 GPa | |
250.0 °C | 76.81 GPa Show Material materials with Schubmodule of 76.81 GPa | |
300.0 °C | 75.05 GPa Show Material materials with Schubmodule of 75.05 GPa | |
350.0 °C | 73.38 GPa Show Material materials with Schubmodule of 73.38 GPa | |
400.0 °C | 71.61 GPa Show Material materials with Schubmodule of 71.61 GPa | |
450.0 °C | 69.75 GPa Show Material materials with Schubmodule of 69.75 GPa | |
500.0 °C | 67.98 GPa Show Material materials with Schubmodule of 67.98 GPa | |
550.0 °C | 66.22 GPa Show Material materials with Schubmodule of 66.22 GPa | |
600.0 °C | 64.35 GPa Show Material materials with Schubmodule of 64.35 GPa | |
Streckgrenze | 20.0 °C | 270 - 285 MPa Show Material materials with Streckgrenze of 270 - 285 MPa |
100.0 °C | 250 - 265 MPa Show Material materials with Streckgrenze of 250 - 265 MPa | |
150.0 °C | 237 - 252 MPa Show Material materials with Streckgrenze of 237 - 252 MPa | |
200.0 °C | 224 - 240 MPa Show Material materials with Streckgrenze of 224 - 240 MPa | |
250.0 °C | 205 - 220 MPa Show Material materials with Streckgrenze of 205 - 220 MPa | |
300.0 °C | 173 - 195 MPa Show Material materials with Streckgrenze of 173 - 195 MPa | |
350.0 °C | 159 - 185 MPa Show Material materials with Streckgrenze of 159 - 185 MPa | |
400.0 °C | 156 - 175 MPa Show Material materials with Streckgrenze of 156 - 175 MPa | |
450.0 °C | 150 - 170 MPa Show Material materials with Streckgrenze of 150 - 170 MPa | |
500.0 °C | 146 - 165 MPa Show Material materials with Streckgrenze of 146 - 165 MPa | |
Streckgrenze Rp 0,2 | 20.0 °C | 270 - 280 MPa Show Material materials with Streckgrenze Rp 0,2 of 270 - 280 MPa |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 270 - 280 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 270 - 280 MPa |
Zugfestigkeit | 20.0 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit of 450 - 600 MPa |
Zugfestigkeit, transversal | 20.0 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit, transversal of 450 - 600 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100.0 °C | 1.05E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44E-5 1/K | ||
Max. Betriebstemperatur, lang | 200 - 550 °C Show Material materials with Max. Betriebstemperatur, lang of 200 - 550 °C | ||
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Molybdenum Steel | |
Spezifische Wärmekapazität | -100.0 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | ||
Temperaturleitfähigkeit | 20.0 °C | 14.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 14.4 mm²/s | |
100.0 °C | 13.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 13.2 mm²/s | ||
200.0 °C | 11.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.7 mm²/s | ||
300.0 °C | 10.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.3 mm²/s | ||
400.0 °C | 9 mm²/s Show Material materials with Temperaturleitfähigkeit of 9 mm²/s | ||
500.0 °C | 7.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.5 mm²/s | ||
600.0 °C | 6 mm²/s Show Material materials with Temperaturleitfähigkeit of 6 mm²/s | ||
Wärmeleitfähigkeit | 20.0 °C | 52.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 52.1 W/(m·K) | |
100.0 °C | 51.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 51.2 W/(m·K) | ||
200.0 °C | 48.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 48.7 W/(m·K) | ||
300.0 °C | 45.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.5 W/(m·K) | ||
400.0 °C | 42.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42.3 W/(m·K) | ||
500.0 °C | 39.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.1 W/(m·K) | ||
600.0 °C | 36 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 2E-7 - 2.16E-7 Ω·m Show Material materials with spezifischer Widerstand of 2E-7 - 2.16E-7 Ω·m |
50.0 °C | 2.37E-7 Ω·m Show Material materials with spezifischer Widerstand of 2.37E-7 Ω·m | |
100.0 °C | 2.5E-7 - 2.68E-7 Ω·m Show Material materials with spezifischer Widerstand of 2.5E-7 - 2.68E-7 Ω·m | |
150.0 °C | 3.02E-7 Ω·m Show Material materials with spezifischer Widerstand of 3.02E-7 Ω·m | |
200.0 °C | 3.24E-7 - 3.39E-7 Ω·m Show Material materials with spezifischer Widerstand of 3.24E-7 - 3.39E-7 Ω·m | |
250.0 °C | 3.8E-7 Ω·m Show Material materials with spezifischer Widerstand of 3.8E-7 Ω·m | |
300.0 °C | 4.12E-7 - 4.25E-7 Ω·m Show Material materials with spezifischer Widerstand of 4.12E-7 - 4.25E-7 Ω·m | |
350.0 °C | 4.74E-7 Ω·m Show Material materials with spezifischer Widerstand of 4.74E-7 Ω·m | |
400.0 °C | 5.14E-7 - 5.27E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.14E-7 - 5.27E-7 Ω·m | |
450.0 °C | 5.83E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.83E-7 Ω·m | |
500.0 °C | 6.33E-7 - 6.42E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.33E-7 - 6.42E-7 Ω·m | |
550.0 °C | 7.08E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.08E-7 Ω·m | |
600.0 °C | 7.69E-7 - 7.78E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.69E-7 - 7.78E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.04 % Show Material materials with Aluminium of 0.04 % |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % |
Kohlenstoff | 0.12 - 0.2 % Show Material materials with Kohlenstoff of 0.12 - 0.2 % |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % |
Mangan | 0.4 - 0.9 % Show Material materials with Mangan of 0.4 - 0.9 % |
Molybdän | 0.25 - 0.35 % Show Material materials with Molybdän of 0.25 - 0.35 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.02 % Show Material materials with Schwefel of 0.02 % |
Silizium | 0.35 % Show Material materials with Silizium of 0.35 % |