Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 21 - 24 % Show Material materials with Dehnung of 21 - 24 % | |
Elastizitätsmodul | 23.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel |
Poissonzahl | 23.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel |
Schubmodule | 23.0 °C | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel |
Streckgrenze | 20.0 °C | 265 - 285 MPa Show Material materials with Streckgrenze of 265 - 285 MPa | |
200.0 °C | 206 MPa Show Material materials with Streckgrenze of 206 MPa | ||
250.0 °C | 186 MPa Show Material materials with Streckgrenze of 186 MPa | ||
300.0 °C | 157 MPa Show Material materials with Streckgrenze of 157 MPa | ||
350.0 °C | 137 MPa Show Material materials with Streckgrenze of 137 MPa | ||
400.0 °C | 118 MPa Show Material materials with Streckgrenze of 118 MPa | ||
Streckgrenze Rp 0,2 | 20.0 °C | 255 - 275 MPa Show Material materials with Streckgrenze Rp 0,2 of 255 - 275 MPa | |
50.0 °C | 251 - 276 MPa Show Material materials with Streckgrenze Rp 0,2 of 251 - 276 MPa | ||
100.0 °C | 237 - 259 MPa Show Material materials with Streckgrenze Rp 0,2 of 237 - 259 MPa | ||
150.0 °C | 219 - 240 MPa Show Material materials with Streckgrenze Rp 0,2 of 219 - 240 MPa | ||
200.0 °C | 201 - 221 MPa Show Material materials with Streckgrenze Rp 0,2 of 201 - 221 MPa | ||
250.0 °C | 184 - 202 MPa Show Material materials with Streckgrenze Rp 0,2 of 184 - 202 MPa | ||
300.0 °C | 151 - 166 MPa Show Material materials with Streckgrenze Rp 0,2 of 151 - 166 MPa | ||
350.0 °C | 137 - 153 MPa Show Material materials with Streckgrenze Rp 0,2 of 137 - 153 MPa | ||
400.0 °C | 118 - 144 MPa Show Material materials with Streckgrenze Rp 0,2 of 118 - 144 MPa | ||
Zugfestigkeit | 20.0 °C | 390 - 510 MPa Show Material materials with Zugfestigkeit of 390 - 510 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.32E-5 - 1.38E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32E-5 - 1.38E-5 1/K | Typical for Low Carbon Steel |
Max. Betriebstemperatur | 500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Spezifische Wärmekapazität | 23.0 °C | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | Typical for Low Carbon Steel |
Wärmeleitfähigkeit | 23.0 °C | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
spezifischer Widerstand | 23.0 °C | 1.43E-7 - 1.74E-7 Ω·m Show Material materials with spezifischer Widerstand of 1.43E-7 - 1.74E-7 Ω·m | Typical for Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.02 - 0.06 % Show Material materials with Aluminium of 0.02 - 0.06 % |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % |
Kohlenstoff | 0.18 % Show Material materials with Kohlenstoff of 0.18 % |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % |
Mangan | 0.6 - 1.5 % Show Material materials with Mangan of 0.6 - 1.5 % |
Molybdän | 0.08 % Show Material materials with Molybdän of 0.08 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |
Niobium | 0.03 % Show Material materials with Niobium of 0.03 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.01 - 0.015 % Show Material materials with Schwefel of 0.01 - 0.015 % |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % |
Stickstoff | 0.02 % Show Material materials with Stickstoff of 0.02 % |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % |