EN 10222-5 Grade X2CrNiN18-10 solution annealed (+AT)

View suppliers (3)
Want to keep this datasheet? Save it now in your required format

Description

The austenitic CrNi_steel X2CrNiN18-10 shows by N-alloying an increased yield stress which also persists at higher temperatures. This is used in pressure vessel construction and for leightweight constructions. Improved corrosion resistance due to the N-content. The material is also in sensitized condition resistant to intercrystalline corrosion. To the comparable trademark X 2 CrNiN 18 10 acc. to DIN 17440 : 1985-07 applies: the material is suitable for chemical apparatus engineering owing to its resistance to nitric acid and other oxidizing media. It is approved in pressure vessel construction up to 300 °C., above 300 °C. subject to authorization. The steel is well cold formable and suitable for mirror finishing. Excellent suitability for refrigeration up to -270 °C.due to its low temperature toughness.

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValue

Dichte

20.0 °C

7.9 - 7.93 g/cm³

Show Material materials with Dichte of 7.9 - 7.93 g/cm³

Mechanisch

PropertyTemperatureValueComment

Dehnung

20.0 °C

35 - 45 %

Show Material materials with Dehnung of 35 - 45 %

Elastizitätsmodul

-100.0 °C

206 GPa

Show Material materials with Elastizitätsmodul of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastizitätsmodul of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastizitätsmodul of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastizitätsmodul of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastizitätsmodul of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastizitätsmodul of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastizitätsmodul of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastizitätsmodul of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastizitätsmodul of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastizitätsmodul of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastizitätsmodul of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastizitätsmodul of 120 GPa

Poissonzahl

23.0 °C

0.3 [-]

Show Material materials with Poissonzahl of 0.3 [-]

Typical for Austenitic Stainless Steel

Schubmodule

23.0 °C

77 GPa

Show Material materials with Schubmodule of 77 GPa

Typical for Austenitic Stainless Steel

Streckgrenze Rp 0,2

20.0 °C

270 MPa

Show Material materials with Streckgrenze Rp 0,2 of 270 MPa

Streckgrenze Rp 1,0

20.0 °C

305 MPa

Show Material materials with Streckgrenze Rp 1,0 of 305 MPa

Zugfestigkeit

20.0 °C

550 - 750 MPa

Show Material materials with Zugfestigkeit of 550 - 750 MPa

Thermisch

PropertyTemperatureValueComment

Koeffizient der thermischen Ausdehnung

-100.0 °C

1.49E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2E-5 1/K

Unlock all property charts

Max. Betriebstemperatur, lang

-270 - 300 °C

Show Material materials with Max. Betriebstemperatur, lang of -270 - 300 °C

Schmelzpunkt

1230 - 1480 °C

Show Material materials with Schmelzpunkt of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Spezifische Wärmekapazität

-100.0 °C

440 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 571 J/(kg·K)

Unlock all property charts

Temperaturleitfähigkeit

20.0 °C

3.8 mm²/s

Show Material materials with Temperaturleitfähigkeit of 3.8 mm²/s

100.0 °C

4 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4 mm²/s

200.0 °C

4.2 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4.2 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4.6 mm²/s

400.0 °C

4.8 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4.8 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Temperaturleitfähigkeit of 4.9 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Temperaturleitfähigkeit of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Temperaturleitfähigkeit of 5.3 mm²/s

800.0 °C

5.6 mm²/s

Show Material materials with Temperaturleitfähigkeit of 5.6 mm²/s

900.0 °C

5.9 mm²/s

Show Material materials with Temperaturleitfähigkeit of 5.9 mm²/s

1000.0 °C

6 mm²/s

Show Material materials with Temperaturleitfähigkeit of 6 mm²/s

Unlock all property charts

Wärmeleitfähigkeit

20.0 °C

14.3 - 15 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 14.3 - 15 W/(m·K)

100.0 °C

15.8 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 15.8 W/(m·K)

200.0 °C

17.5 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 17.5 W/(m·K)

300.0 °C

19 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 19 W/(m·K)

400.0 °C

20.5 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 20.5 W/(m·K)

500.0 °C

21.9 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 21.9 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 23.3 W/(m·K)

700.0 °C

24.6 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 24.6 W/(m·K)

800.0 °C

26 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 26 W/(m·K)

900.0 °C

27.4 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 27.4 W/(m·K)

1000.0 °C

28.8 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 28.8 W/(m·K)

Unlock all property charts

Elektrisch

PropertyTemperatureValue

spezifischer Widerstand

20.0 °C

7.1E-7 Ω·m

Show Material materials with spezifischer Widerstand of 7.1E-7 Ω·m

100.0 °C

7.76E-7 Ω·m

Show Material materials with spezifischer Widerstand of 7.76E-7 Ω·m

200.0 °C

8.49E-7 Ω·m

Show Material materials with spezifischer Widerstand of 8.49E-7 Ω·m

300.0 °C

9.14E-7 Ω·m

Show Material materials with spezifischer Widerstand of 9.14E-7 Ω·m

400.0 °C

9.71E-7 Ω·m

Show Material materials with spezifischer Widerstand of 9.71E-7 Ω·m

500.0 °C

1.02E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.02E-6 Ω·m

600.0 °C

1.07E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.07E-6 Ω·m

700.0 °C

1.1E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.1E-6 Ω·m

800.0 °C

1.14E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.14E-6 Ω·m

900.0 °C

1.17E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.17E-6 Ω·m

1000.0 °C

1.19E-6 Ω·m

Show Material materials with spezifischer Widerstand of 1.19E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Chrom

17 - 19.5 %

Show Material materials with Chrom of 17 - 19.5 %

Kohlenstoff

0.03 %

Show Material materials with Kohlenstoff of 0.03 %

Mangan

2 %

Show Material materials with Mangan of 2 %

Nickel

8.5 - 11.5 %

Show Material materials with Nickel of 8.5 - 11.5 %

Phosphor

0.05 %

Show Material materials with Phosphor of 0.05 %

Schwefel

0.015 %

Show Material materials with Schwefel of 0.015 %

Silizium

1 %

Show Material materials with Silizium of 1 %

Stickstoff

0.12 - 0.22 %

Show Material materials with Stickstoff of 0.12 - 0.22 %