Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | Typical for Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 11.8 % Show Material materials with Dehnung of 11.8 % | Predicted Value, A80 | ||||
12.7 % Show Material materials with Dehnung of 12.7 % | Predicted Value, A200 | |||||
14.7 % Show Material materials with Dehnung of 14.7 % | Predicted Value, Transverse | |||||
17.9 % Show Material materials with Dehnung of 17.9 % | Predicted Value, A5 | |||||
17.9 % Show Material materials with Dehnung of 17.9 % | Predicted Value, A50 | |||||
18.4 % Show Material materials with Dehnung of 18.4 % | Predicted Value, A80 Transverse | |||||
20 °C | 14 % Show Material materials with Dehnung of 14 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
Elastizitätsmodul | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel | ||||
Flächenreduzierung | 40.3 % Show Material materials with Flächenreduzierung of 40.3 % | Predicted Value | ||||
44.8 % Show Material materials with Flächenreduzierung of 44.8 % | Predicted Value, Transverse | |||||
Poissonzahl | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel | ||||
Scherfestigkeit | 575.7 MPa Show Material materials with Scherfestigkeit of 575.7 MPa | Predicted Value | ||||
Schubmodule | 79.8 GPa Show Material materials with Schubmodule of 79.8 GPa | Predicted Value | ||||
Streckgrenze | 309 MPa Show Material materials with Streckgrenze of 309 MPa | Predicted Value, RP1 | ||||
329.7 MPa Show Material materials with Streckgrenze of 329.7 MPa | Predicted Value, RP1 Transverse | |||||
503.5 MPa Show Material materials with Streckgrenze of 503.5 MPa | Predicted Value, RP02 Transverse | |||||
541.7 MPa Show Material materials with Streckgrenze of 541.7 MPa | Predicted Value, RP05 | |||||
542.7 MPa Show Material materials with Streckgrenze of 542.7 MPa | Predicted Value, Transverse | |||||
587.5 MPa Show Material materials with Streckgrenze of 587.5 MPa | Predicted Value, RP02 | |||||
722.2 MPa Show Material materials with Streckgrenze of 722.2 MPa | Predicted Value, RP002 | |||||
20 °C | 630 MPa Show Material materials with Streckgrenze of 630 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 650 MPa Show Material materials with Streckgrenze of 650 MPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
20 °C | 670 MPa Show Material materials with Streckgrenze of 670 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 690 MPa Show Material materials with Streckgrenze of 690 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
Zugfestigkeit | 20 °C | 710 - 940 MPa Show Material materials with Zugfestigkeit of 710 - 940 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | |
20 °C | 710 - 930 MPa Show Material materials with Zugfestigkeit of 710 - 930 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 710 - 900 MPa Show Material materials with Zugfestigkeit of 710 - 900 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 760 - 940 MPa Show Material materials with Zugfestigkeit of 760 - 940 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 760 - 930 MPa Show Material materials with Zugfestigkeit of 760 - 930 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 760 - 900 MPa Show Material materials with Zugfestigkeit of 760 - 900 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 770 - 940 MPa Show Material materials with Zugfestigkeit of 770 - 940 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 770 - 930 MPa Show Material materials with Zugfestigkeit of 770 - 930 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat | ||
20 °C | 770 - 900 MPa Show Material materials with Zugfestigkeit of 770 - 900 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 11.9 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 11.9 1/K | Predicted Value |
Spezifische Wärmekapazität | 441.6 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 441.6 J/(kg·K) | Predicted Value |
Wärmeleitfähigkeit | 35.86 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.86 W/(m·K) | Predicted Value |
Elektrisch
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bor | 0.005 % Show Material materials with Bor of 0.005 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Chrom | 1.5 % Show Material materials with Chrom of 1.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Kohlenstoff | 0.2 % Show Material materials with Kohlenstoff of 0.2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Kupfer | 0.5 % Show Material materials with Kupfer of 0.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Mangan | 1.7 % Show Material materials with Mangan of 1.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Molybdän | 0.7 % Show Material materials with Molybdän of 0.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Nickel | 2 % Show Material materials with Nickel of 2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Niobium | 0.06 % Show Material materials with Niobium of 0.06 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Silizium | 0.8 % Show Material materials with Silizium of 0.8 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Stickstoff | 0.015 % Show Material materials with Stickstoff of 0.015 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Titan | 0.05 % Show Material materials with Titan of 0.05 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Vanadium | 0.12 % Show Material materials with Vanadium of 0.12 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Zirkonium | 0.15 % Show Material materials with Zirkonium of 0.15 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6 | Sheet, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |