Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.92 g/cm³ Show Material materials with Dichte of 7.92 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | -100.0 °C | 206 GPa Show Material materials with Elastizitätsmodul of 206 GPa | |
20.0 °C | 190 - 200 GPa Show Material materials with Elastizitätsmodul of 190 - 200 GPa | ||
100.0 °C | 190 GPa Show Material materials with Elastizitätsmodul of 190 GPa | ||
200.0 °C | 182 GPa Show Material materials with Elastizitätsmodul of 182 GPa | ||
300.0 °C | 174 GPa Show Material materials with Elastizitätsmodul of 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Elastizitätsmodul of 166 GPa | ||
500.0 °C | 158 GPa Show Material materials with Elastizitätsmodul of 158 GPa | ||
600.0 °C | 150 GPa Show Material materials with Elastizitätsmodul of 150 GPa | ||
700.0 °C | 142 GPa Show Material materials with Elastizitätsmodul of 142 GPa | ||
800.0 °C | 134 GPa Show Material materials with Elastizitätsmodul of 134 GPa | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel |
Schubmodule | 20.0 °C | 73 - 78 GPa Show Material materials with Schubmodule of 73 - 78 GPa | |
Zugfestigkeit | 20.0 °C | 1500 - 2275 MPa Show Material materials with Zugfestigkeit of 1500 - 2275 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | -100.0 °C | 1.49E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49E-5 1/K |
20.0 °C | 1.61E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.61E-5 1/K | |
100.0 °C | 1.67E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.67E-5 1/K | |
200.0 °C | 1.72E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.72E-5 1/K | |
300.0 °C | 1.77E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.77E-5 1/K | |
400.0 °C | 1.81E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.81E-5 1/K | |
500.0 °C | 1.84E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.84E-5 1/K | |
600.0 °C | 1.88E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.88E-5 1/K | |
700.0 °C | 1.91E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.91E-5 1/K | |
800.0 °C | 1.94E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.94E-5 1/K | |
Max. Betriebstemperatur, lang | -150 - 350 °C Show Material materials with Max. Betriebstemperatur, lang of -150 - 350 °C | |
Spezifische Wärmekapazität | -100.0 °C | 440 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 440 J/(kg·K) |
20.0 °C | 472 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 472 J/(kg·K) | |
100.0 °C | 487 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 487 J/(kg·K) | |
200.0 °C | 503 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 503 J/(kg·K) | |
300.0 °C | 512 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 512 J/(kg·K) | |
400.0 °C | 520 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 520 J/(kg·K) | |
500.0 °C | 530 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 530 J/(kg·K) | |
600.0 °C | 541 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 541 J/(kg·K) | |
700.0 °C | 551 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 551 J/(kg·K) | |
800.0 °C | 559 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 559 J/(kg·K) | |
Temperaturleitfähigkeit | -100.0 °C | 3.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 3.7 mm²/s |
20.0 °C | 3.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 3.9 mm²/s | |
100.0 °C | 4.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.3 mm²/s | |
200.0 °C | 4.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.3 mm²/s | |
300.0 °C | 4.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.6 mm²/s | |
400.0 °C | 4.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.7 mm²/s | |
500.0 °C | 4.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.9 mm²/s | |
600.0 °C | 5 mm²/s Show Material materials with Temperaturleitfähigkeit of 5 mm²/s | |
700.0 °C | 5.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.3 mm²/s | |
800.0 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | |
Wärmeleitfähigkeit | -100.0 °C | 11.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 11.7 W/(m·K) |
20.0 °C | 14.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 14.5 W/(m·K) | |
100.0 °C | 16 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 16 W/(m·K) | |
200.0 °C | 17.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 17.6 W/(m·K) | |
300.0 °C | 19.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 19.1 W/(m·K) | |
400.0 °C | 20.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 20.4 W/(m·K) | |
500.0 °C | 21.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 21.9 W/(m·K) | |
600.0 °C | 23.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 23.3 W/(m·K) | |
700.0 °C | 24.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 24.7 W/(m·K) | |
800.0 °C | 26.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 26.1 W/(m·K) | |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | -100.0 °C | 5.86E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.86E-7 Ω·m |
20.0 °C | 6.92E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.92E-7 Ω·m | |
100.0 °C | 7.58E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.58E-7 Ω·m | |
200.0 °C | 8.36E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.36E-7 Ω·m | |
300.0 °C | 9.07E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.07E-7 Ω·m | |
400.0 °C | 9.73E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.73E-7 Ω·m | |
500.0 °C | 1.02E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.02E-6 Ω·m | |
600.0 °C | 1.06E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.06E-6 Ω·m | |
700.0 °C | 1.1E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.1E-6 Ω·m | |
800.0 °C | 1.13E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.13E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.7 - 1.5 % Show Material materials with Aluminium of 0.7 - 1.5 % |
Chrom | 16 - 18 % Show Material materials with Chrom of 16 - 18 % |
Kohlenstoff | 0.09 % Show Material materials with Kohlenstoff of 0.09 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Nickel | 6.5 - 7.8 % Show Material materials with Nickel of 6.5 - 7.8 % |
Phosphor | 0.04 % Show Material materials with Phosphor of 0.04 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 0.7 % Show Material materials with Silizium of 0.7 % |
Technological properties
Property | ||
---|---|---|
Features | Spring |