Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.9 g/cm³ Show Material materials with Dichte of 8.9 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 10 - 14 % Show Material materials with Dehnung of 10 - 14 % |
Dehnung, transversal | 20.0 °C | 14 % Show Material materials with Dehnung, transversal of 14 % |
Elastizitätsmodul | -253.0 °C | 153 GPa Show Material materials with Elastizitätsmodul of 153 GPa |
-195.0 °C | 148 GPa Show Material materials with Elastizitätsmodul of 148 GPa | |
-100.0 °C | 142 GPa Show Material materials with Elastizitätsmodul of 142 GPa | |
20.0 °C | 130 GPa Show Material materials with Elastizitätsmodul of 130 GPa | |
50.0 °C | 129 GPa Show Material materials with Elastizitätsmodul of 129 GPa | |
100.0 °C | 128 GPa Show Material materials with Elastizitätsmodul of 128 GPa | |
150.0 °C | 127 GPa Show Material materials with Elastizitätsmodul of 127 GPa | |
200.0 °C | 125 GPa Show Material materials with Elastizitätsmodul of 125 GPa | |
250.0 °C | 122 GPa Show Material materials with Elastizitätsmodul of 122 GPa | |
300.0 °C | 121 GPa Show Material materials with Elastizitätsmodul of 121 GPa | |
Elongation A10 | 20.0 °C | 8 % Show Material materials with Elongation A10 of 8 % |
Elongation A100 | 20.0 °C | 6 % Show Material materials with Elongation A100 of 6 % |
Elongation A11.3 | 20.0 °C | 8 % Show Material materials with Elongation A11.3 of 8 % |
Härte, Vickers | 20.0 °C | 120 [-] Show Material materials with Härte, Vickers of 120 [-] |
Streckgrenze Rp 0,2 | 20.0 °C | 150 - 250 MPa Show Material materials with Streckgrenze Rp 0,2 of 150 - 250 MPa |
50.0 °C | 250 MPa Show Material materials with Streckgrenze Rp 0,2 of 250 MPa | |
100.0 °C | 235 MPa Show Material materials with Streckgrenze Rp 0,2 of 235 MPa | |
150.0 °C | 225 MPa Show Material materials with Streckgrenze Rp 0,2 of 225 MPa | |
200.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 0,2 of 220 MPa | |
250.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 0,2 of 210 MPa | |
300.0 °C | 205 MPa Show Material materials with Streckgrenze Rp 0,2 of 205 MPa | |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 250 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 250 MPa |
50.0 °C | 250 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 250 MPa | |
100.0 °C | 235 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 235 MPa | |
150.0 °C | 210 - 225 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 210 - 225 MPa | |
200.0 °C | 205 - 220 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 205 - 220 MPa | |
250.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 210 MPa | |
300.0 °C | 205 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 205 MPa | |
Zugfestigkeit | 20.0 °C | 350 MPa Show Material materials with Zugfestigkeit of 350 MPa |
Zugfestigkeit, transversal | 20.0 °C | 350 MPa Show Material materials with Zugfestigkeit, transversal of 350 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.4E-5 - 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4E-5 - 1.8E-5 1/K | Typical for Wrought Copper Nickel Grade |
Schmelzpunkt | 915 - 1240 °C Show Material materials with Schmelzpunkt of 915 - 1240 °C | Typical for Wrought Copper Nickel Grade | |
Spezifische Wärmekapazität | 20.0 °C | 380 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 380 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 50.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 50.2 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Blei | 0.02 % Show Material materials with Blei of 0.02 % |
Eisen | 1 - 2 % Show Material materials with Eisen of 1 - 2 % |
Kobalt | 0.1 % Show Material materials with Kobalt of 0.1 % |
Kohlenstoff | 0.05 % Show Material materials with Kohlenstoff of 0.05 % |
Mangan | 0.5 - 1 % Show Material materials with Mangan of 0.5 - 1 % |
Nickel | 9 - 11 % Show Material materials with Nickel of 9 - 11 % |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % |
Schwefel | 0.05 % Show Material materials with Schwefel of 0.05 % |
Zink | 0.5 % Show Material materials with Zink of 0.5 % |
Zinn | 0.03 % Show Material materials with Zinn of 0.03 % |