Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.4 g/cm³ Show Material materials with Dichte of 8.4 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 20 - 25 % Show Material materials with Dehnung of 20 - 25 % | |
Elastizitätsmodul | 20.0 °C | 102 GPa Show Material materials with Elastizitätsmodul of 102 GPa | |
Elongation A100 | 20.0 °C | 10 % Show Material materials with Elongation A100 of 10 % | |
Elongation A11.3 | 20.0 °C | 15 % Show Material materials with Elongation A11.3 of 15 % | |
Schubmodule | 23.0 °C | 40 GPa Show Material materials with Schubmodule of 40 GPa | Typical for Wrought Copper Brass |
Streckgrenze Rp 0,2 | 20.0 °C | 150 - 300 MPa Show Material materials with Streckgrenze Rp 0,2 of 150 - 300 MPa | |
Zugfestigkeit | 20.0 °C | 360 MPa Show Material materials with Zugfestigkeit of 360 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 - 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 2.1E-5 1/K | Typical for Wrought Copper Brass |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 20.0 °C | 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 377 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 109 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 109 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.39E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 1.39E+7 S/m |
Specific Electrical conductivity | 24 % IACS Show Material materials with Specific Electrical conductivity of 24 % IACS |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.05 % Show Material materials with Aluminium of 0.05 % |
Blei | 0.8 - 1.6 % Show Material materials with Blei of 0.8 - 1.6 % |
Eisen | 0.2 % Show Material materials with Eisen of 0.2 % |
Kupfer | 60 - 61 % Show Material materials with Kupfer of 60 - 61 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |
Zinn | 0.2 % Show Material materials with Zinn of 0.2 % |