EN 12166 Grade CuSn4 H230

View suppliers (9)
Want to keep this datasheet? Save it now in your required format

Description

CuSn4, mat. No. CW450K, is comparable to the DIN-make CuSn4, mat. No. 2.1016, acc. to DIN 17662 : 1983-12. The material is specified by a favorable combination of very good cold formability with strength and hardness. It is corrosion resistant, good soft and hard solderable and shows still good electrical conductivity. Properties of the CuSn-alloy are predominantly determined by the tin-content. The alloy is unhardenable, only work hardening is feasible. Tensile strength, yield point and hardness increase according to the rising cold forming grade, elongation after fracture decreases. Electrical and thermal conductivity are lower than for pure copper. Very high resistance to corrosion, particularly to atmospheric influences, seawater, sulfite liquor, carbonated and salted mine water. The alloys are stress corrosion-proof. Processing properties: warm forming: limited cold forming: very good machinability: moderately to hardly hard soldering: very good soft soldering: very good gas welding: medium arc welding: medium TIG-welding: good MIG_welding: good resistance welding: good electron beam welding: good sticking: suitable burnishing: good mechanical burnishing: good electrolytical/chemical burnishing: good galvanizing: very good suitability for dip tinning: very good Appliction: CuSn4 is predominantly used in the form of strips for all types of springs with mean requirements, such as connectors, electrographic springs for contacts and earthing contacts, clamp-connenctions for radio, TV and video, receptacles for electronical assemblies, for pushbutton shifting springs and locking clamps, spring rings as well as for textile machine components. For the electrolytically tinned strip the coatings (Sn bright, Sn matt, Sn fuzed, SnPb) are listed by the application (better solderability, better corrosion resistance, reduction of the electrical contact resistance, better appearance) in the DIN EN 14436 : 2004-11 (Table 5)

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValue

Dichte

20.0 °C

8.7 - 8.9 g/cm³

Show Material materials with Dichte of 8.7 - 8.9 g/cm³

Mechanisch

PropertyTemperatureValue

Elastizitätsmodul

20.0 °C

120 GPa

Show Material materials with Elastizitätsmodul of 120 GPa

Härte, Vickers

20.0 °C

230 [-]

Show Material materials with Härte, Vickers of 230 [-]

Poissonzahl

20.0 °C

0.34 [-]

Show Material materials with Poissonzahl of 0.34 [-]

Thermisch

PropertyTemperatureValue

Koeffizient der thermischen Ausdehnung

100.0 °C

1.78E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.78E-5 1/K

200.0 °C

1.82E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.82E-5 1/K

300.0 °C

1.9E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9E-5 1/K

650.0 °C

2.06E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.06E-5 1/K

800.0 °C

2.05E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.05E-5 1/K

Spezifische Wärmekapazität

20.0 °C

377 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 377 J/(kg·K)

Wärmeleitfähigkeit

20.0 °C

90 - 100 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 90 - 100 W/(m·K)

200.0 °C

120 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 120 W/(m·K)

Unlock all property charts

Elektrisch

PropertyTemperatureValue

Elektrische Leitfähigkeit

20.0 °C

1.18E+7 - 1.20E+7 S/m

Show Material materials with Elektrische Leitfähigkeit of 1.18E+7 - 1.20E+7 S/m

200.0 °C

1.07E+7 S/m

Show Material materials with Elektrische Leitfähigkeit of 1.07E+7 S/m

Unlock all property charts

Specific Electrical conductivity

21 % IACS

Show Material materials with Specific Electrical conductivity of 21 % IACS

spezifischer Widerstand

20.0 °C

8.5E-8 Ω·m

Show Material materials with spezifischer Widerstand of 8.5E-8 Ω·m

200.0 °C

9.3E-8 Ω·m

Show Material materials with spezifischer Widerstand of 9.3E-8 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Blei

0.02 %

Show Material materials with Blei of 0.02 %

Eisen

0.1 %

Show Material materials with Eisen of 0.1 %

Nickel

0.2 %

Show Material materials with Nickel of 0.2 %

Phosphor

0.01 - 0.4 %

Show Material materials with Phosphor of 0.01 - 0.4 %

Zink

0.2 %

Show Material materials with Zink of 0.2 %

Zinn

3.5 - 4.5 %

Show Material materials with Zinn of 3.5 - 4.5 %