Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.33 g/cm³ Show Material materials with Dichte of 8.33 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 40 - 55 % Show Material materials with Dehnung of 40 - 55 % |
100.0 °C | 50 - 56 % Show Material materials with Dehnung of 50 - 56 % | |
150.0 °C | 56 % Show Material materials with Dehnung of 56 % | |
200.0 °C | 43 - 50 % Show Material materials with Dehnung of 43 - 50 % | |
250.0 °C | 22 % Show Material materials with Dehnung of 22 % | |
300.0 °C | 42 % Show Material materials with Dehnung of 42 % | |
400.0 °C | 23 % Show Material materials with Dehnung of 23 % | |
500.0 °C | 35 % Show Material materials with Dehnung of 35 % | |
Elastizitätsmodul | 20.0 °C | 110 - 112 GPa Show Material materials with Elastizitätsmodul of 110 - 112 GPa |
50.0 °C | 110 - 130 GPa Show Material materials with Elastizitätsmodul of 110 - 130 GPa | |
100.0 °C | 108 - 128 GPa Show Material materials with Elastizitätsmodul of 108 - 128 GPa | |
150.0 °C | 107 - 126 GPa Show Material materials with Elastizitätsmodul of 107 - 126 GPa | |
200.0 °C | 106 - 123 GPa Show Material materials with Elastizitätsmodul of 106 - 123 GPa | |
250.0 °C | 105 - 120 GPa Show Material materials with Elastizitätsmodul of 105 - 120 GPa | |
300.0 °C | 118 GPa Show Material materials with Elastizitätsmodul of 118 GPa | |
350.0 °C | 115 GPa Show Material materials with Elastizitätsmodul of 115 GPa | |
400.0 °C | 112 GPa Show Material materials with Elastizitätsmodul of 112 GPa | |
450.0 °C | 109 GPa Show Material materials with Elastizitätsmodul of 109 GPa | |
500.0 °C | 105 GPa Show Material materials with Elastizitätsmodul of 105 GPa | |
Flächenreduzierung | 100.0 °C | 69 % Show Material materials with Flächenreduzierung of 69 % |
150.0 °C | 63 % Show Material materials with Flächenreduzierung of 63 % | |
200.0 °C | 37 % Show Material materials with Flächenreduzierung of 37 % | |
250.0 °C | 23 % Show Material materials with Flächenreduzierung of 23 % | |
Härte, Brinell | 20.0 °C | 65 - 95 [-] Show Material materials with Härte, Brinell of 65 - 95 [-] |
Härte, Vickers | 20.0 °C | 60 - 110 [-] Show Material materials with Härte, Vickers of 60 - 110 [-] |
Schubmodule | 20.0 °C | 42 GPa Show Material materials with Schubmodule of 42 GPa |
Streckgrenze Rp 0,2 | 20.0 °C | 89 - 150 MPa Show Material materials with Streckgrenze Rp 0,2 of 89 - 150 MPa |
100.0 °C | 180 MPa Show Material materials with Streckgrenze Rp 0,2 of 180 MPa | |
150.0 °C | 180 MPa Show Material materials with Streckgrenze Rp 0,2 of 180 MPa | |
200.0 °C | 65 - 175 MPa Show Material materials with Streckgrenze Rp 0,2 of 65 - 175 MPa | |
250.0 °C | 170 MPa Show Material materials with Streckgrenze Rp 0,2 of 170 MPa | |
300.0 °C | 60 MPa Show Material materials with Streckgrenze Rp 0,2 of 60 MPa | |
400.0 °C | 55 MPa Show Material materials with Streckgrenze Rp 0,2 of 55 MPa | |
Streckgrenze Rp 1,0 | 100.0 °C | 195 MPa Show Material materials with Streckgrenze Rp 1,0 of 195 MPa |
150.0 °C | 195 MPa Show Material materials with Streckgrenze Rp 1,0 of 195 MPa | |
200.0 °C | 195 MPa Show Material materials with Streckgrenze Rp 1,0 of 195 MPa | |
250.0 °C | 190 MPa Show Material materials with Streckgrenze Rp 1,0 of 190 MPa | |
Zugfestigkeit | 20.0 °C | 340 - 420 MPa Show Material materials with Zugfestigkeit of 340 - 420 MPa |
100.0 °C | 395 - 410 MPa Show Material materials with Zugfestigkeit of 395 - 410 MPa | |
150.0 °C | 385 MPa Show Material materials with Zugfestigkeit of 385 MPa | |
200.0 °C | 365 - 375 MPa Show Material materials with Zugfestigkeit of 365 - 375 MPa | |
250.0 °C | 310 MPa Show Material materials with Zugfestigkeit of 310 MPa | |
300.0 °C | 355 MPa Show Material materials with Zugfestigkeit of 355 MPa | |
400.0 °C | 280 MPa Show Material materials with Zugfestigkeit of 280 MPa | |
500.0 °C | 130 MPa Show Material materials with Zugfestigkeit of 130 MPa | |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 200.0 °C | 1.85E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.85E-5 1/K | |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 20.0 °C | 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 377 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 100 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 100 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.34E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 1.34E+7 S/m |
spezifischer Widerstand | 20.0 °C | 7.5E-8 Ω·m Show Material materials with spezifischer Widerstand of 7.5E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 1.8 - 2.3 % Show Material materials with Aluminium of 1.8 - 2.3 % |
Arsen | 0.02 - 0.06 % Show Material materials with Arsen of 0.02 - 0.06 % |
Blei | 0.05 - 0.5 % Show Material materials with Blei of 0.05 - 0.5 % |
Eisen | 0.07 % Show Material materials with Eisen of 0.07 % |
Kupfer | 76 - 79 % Show Material materials with Kupfer of 76 - 79 % |
Magnesium | 5E-3 % Show Material materials with Magnesium of 5E-3 % |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % |
Nickel | 0.1 % Show Material materials with Nickel of 0.1 % |
Phosphor | 0.01 % Show Material materials with Phosphor of 0.01 % |