Allgemein
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Creep strength 10^4 cycles | 600.0 °C | 241 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 241 MPa | at 10000h |
610.0 °C | 231 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 231 MPa | at 10000h | |
620.0 °C | 221 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 221 MPa | at 10000h | |
630.0 °C | 210 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 210 MPa | at 10000h | |
640.0 °C | 198 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 198 MPa | at 10000h | |
650.0 °C | 184 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 184 MPa | at 10000h | |
660.0 °C | 167 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 167 MPa | at 10000h | |
670.0 °C | 147 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 147 MPa | at 10000h | |
680.0 °C | 124 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 124 MPa | at 10000h | |
690.0 °C | 102 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 102 MPa | at 10000h | |
700.0 °C | 86 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 86 MPa | at 10000h | |
710.0 °C | 75 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 75 MPa | at 10000h | |
720.0 °C | 67 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 67 MPa | at 10000h | |
730.0 °C | 61 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 61 MPa | at 10000h | |
740.0 °C | 55 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 55 MPa | at 10000h | |
750.0 °C | 51 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 51 MPa | at 10000h | |
760.0 °C | 46 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 46 MPa | at 10000h | |
770.0 °C | 42 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 42 MPa | at 10000h | |
780.0 °C | 38 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 38 MPa | at 10000h | |
790.0 °C | 34 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 34 MPa | at 10000h | |
Creep strength 10^5 cycles | 600.0 °C | 199 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 199 MPa | at 100000h |
610.0 °C | 185 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 185 MPa | at 100000h | |
620.0 °C | 167 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 167 MPa | at 100000h | |
630.0 °C | 147 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 147 MPa | at 100000h | |
640.0 °C | 122 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 122 MPa | at 100000h | |
650.0 °C | 100 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 100 MPa | at 100000h | |
660.0 °C | 84 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 84 MPa | at 100000h | |
670.0 °C | 74 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 74 MPa | at 100000h | |
680.0 °C | 66 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 66 MPa | at 100000h | |
690.0 °C | 59 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 59 MPa | at 100000h | |
700.0 °C | 54 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 54 MPa | at 100000h | |
710.0 °C | 49 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 49 MPa | at 100000h | |
720.0 °C | 45 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 45 MPa | at 100000h | |
730.0 °C | 40 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 40 MPa | at 100000h | |
740.0 °C | 36 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 36 MPa | at 100000h | |
750.0 °C | 30 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 30 MPa | at 100000h | |
Creep strength 25x10^4 cycles | 600.0 °C | 177 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 177 MPa | at 250000h |
610.0 °C | 158 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 158 MPa | at 250000h | |
620.0 °C | 134 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 134 MPa | at 250000h | |
630.0 °C | 109 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 109 MPa | at 250000h | |
640.0 °C | 90 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 90 MPa | at 250000h | |
650.0 °C | 78 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 78 MPa | at 250000h | |
660.0 °C | 69 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 69 MPa | at 250000h | |
670.0 °C | 52 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 52 MPa | at 250000h | |
680.0 °C | 56 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 56 MPa | at 250000h | |
700.0 °C | 46 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 46 MPa | at 250000h | |
710.0 °C | 42 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 42 MPa | at 250000h | |
720.0 °C | 37 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 37 MPa | at 250000h | |
730.0 °C | 32 MPa Show Supplier Material materials with Creep strength 25x10^4 cycles of 32 MPa | at 250000h | |
Dehnung | 23.0 °C | 35 % Show Supplier Material materials with Dehnung of 35 % | min. |
Elastizitätsmodul | 20.0 °C | 192 GPa Show Supplier Material materials with Elastizitätsmodul of 192 GPa | |
100.0 °C | 184 GPa Show Supplier Material materials with Elastizitätsmodul of 184 GPa | ||
200.0 °C | 176 GPa Show Supplier Material materials with Elastizitätsmodul of 176 GPa | ||
300.0 °C | 168 GPa Show Supplier Material materials with Elastizitätsmodul of 168 GPa | ||
400.0 °C | 160 GPa Show Supplier Material materials with Elastizitätsmodul of 160 GPa | ||
500.0 °C | 151 GPa Show Supplier Material materials with Elastizitätsmodul of 151 GPa | ||
600.0 °C | 143 GPa Show Supplier Material materials with Elastizitätsmodul of 143 GPa | ||
700.0 °C | 135 GPa Show Supplier Material materials with Elastizitätsmodul of 135 GPa | ||
800.0 °C | 127 GPa Show Supplier Material materials with Elastizitätsmodul of 127 GPa | ||
900.0 °C | 120 GPa Show Supplier Material materials with Elastizitätsmodul of 120 GPa | ||
Härte, Rockwell B | 23.0 °C | 90 [-] Show Supplier Material materials with Härte, Rockwell B of 90 [-] | max. |
Streckgrenze Rp 0,2 | 20.0 °C | 230 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 230 MPa | min. |
50.0 °C | 213 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 213 MPa | min. | |
100.0 °C | 188 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 188 MPa | min. | |
150.0 °C | 171 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 171 MPa | min. | |
200.0 °C | 161 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 161 MPa | min. | |
250.0 °C | 153 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 153 MPa | min. | |
300.0 °C | 148 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 148 MPa | min. | |
350.0 °C | 145 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 145 MPa | min. | |
400.0 °C | 144 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 144 MPa | min. | |
450.0 °C | 141 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 141 MPa | min. | |
500.0 °C | 139 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 139 MPa | min. | |
550.0 °C | 136 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 136 MPa | min. | |
600.0 °C | 133 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 133 MPa | min. | |
650.0 °C | 130 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 130 MPa | min. | |
700.0 °C | 125 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 125 MPa | min. | |
Streckgrenze Rp0,1 | 20.0 °C | 270 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 270 MPa | min. |
50.0 °C | 254 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 254 MPa | min. | |
100.0 °C | 232 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 232 MPa | min. | |
150.0 °C | 210 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 210 MPa | min. | |
200.0 °C | 195 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 195 MPa | min. | |
250.0 °C | 190 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 190 MPa | min. | |
300.0 °C | 187 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 187 MPa | min. | |
350.0 °C | 184 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 184 MPa | min. | |
400.0 °C | 182 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 182 MPa | min. | |
450.0 °C | 179 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 179 MPa | min. | |
500.0 °C | 178 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 178 MPa | min. | |
550.0 °C | 175 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 175 MPa | min. | |
600.0 °C | 170 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 170 MPa | min. | |
650.0 °C | 165 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 165 MPa | min. | |
700.0 °C | 159 MPa Show Supplier Material materials with Streckgrenze Rp0,1 of 159 MPa | min. | |
Verlängerung A2 | 23.0 °C | 35 % Show Supplier Material materials with Verlängerung A2 of 35 % | min. |
Zugfestigkeit | 23.0 °C | 540 - 740 MPa Show Supplier Material materials with Zugfestigkeit of 540 - 740 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.5E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.5E-5 1/K | for 30°C to the mentioned temperature |
200.0 °C | 1.6E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | for 30°C to the mentioned temperature | |
300.0 °C | 1.7E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | for 30°C to the mentioned temperature | |
400.0 °C | 1.8E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | for 30°C to the mentioned temperature | |
500.0 °C | 1.85E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.85E-5 1/K | for 30°C to the mentioned temperature | |
600.0 °C | 1.9E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.9E-5 1/K | for 30°C to the mentioned temperature | |
700.0 °C | 1.9E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.9E-5 1/K | for 30°C to the mentioned temperature | |
800.0 °C | 1.95E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.95E-5 1/K | for 30°C to the mentioned temperature | |
900.0 °C | 2E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2E-5 1/K | for 30°C to the mentioned temperature | |
Spezifische Wärmekapazität | 100.0 °C | 505 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 505 J/(kg·K) | for 20°C to the mentioned temperature |
200.0 °C | 530 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 530 J/(kg·K) | for 20°C to the mentioned temperature | |
300.0 °C | 540 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 540 J/(kg·K) | for 20°C to the mentioned temperature | |
400.0 °C | 545 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 545 J/(kg·K) | for 20°C to the mentioned temperature | |
500.0 °C | 555 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 555 J/(kg·K) | for 20°C to the mentioned temperature | |
600.0 °C | 560 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 560 J/(kg·K) | for 20°C to the mentioned temperature | |
700.0 °C | 565 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 565 J/(kg·K) | for 20°C to the mentioned temperature | |
800.0 °C | 575 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 575 J/(kg·K) | for 20°C to the mentioned temperature | |
900.0 °C | 580 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 580 J/(kg·K) | for 20°C to the mentioned temperature | |
1000.0 °C | 585 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 585 J/(kg·K) | for 20°C to the mentioned temperature | |
Wärmeleitfähigkeit | 20.0 °C | 13 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 13 W/(m·K) | |
100.0 °C | 14 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 14 W/(m·K) | ||
200.0 °C | 15 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 15 W/(m·K) | ||
300.0 °C | 17 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 17 W/(m·K) | ||
400.0 °C | 19 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 19 W/(m·K) | ||
500.0 °C | 20 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 20 W/(m·K) | ||
600.0 °C | 22 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 22 W/(m·K) | ||
700.0 °C | 23 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 23 W/(m·K) | ||
800.0 °C | 24 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 24 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 7.4E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 7.4E-7 Ω·m |
100.0 °C | 8E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 8E-7 Ω·m | |
200.0 °C | 8.8E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 8.8E-7 Ω·m | |
300.0 °C | 9.4E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 9.4E-7 Ω·m | |
400.0 °C | 1E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1E-6 Ω·m | |
500.0 °C | 1.05E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1.05E-6 Ω·m | |
600.0 °C | 1.09E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1.09E-6 Ω·m | |
700.0 °C | 1.13E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1.13E-6 Ω·m | |
800.0 °C | 1.16E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1.16E-6 Ω·m | |
900.0 °C | 1.18E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1.18E-6 Ω·m | |
1000.0 °C | 1.2E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1.2E-6 Ω·m | |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Bor | 5E-3 % Show Supplier Material materials with Bor of 5E-3 % | ||
Chrom | 15 % Show Supplier Material materials with Chrom of 15 % | ||
Eisen | Balance | ||
Kohlenstoff | 0.1 % Show Supplier Material materials with Kohlenstoff of 0.1 % | ||
Mangan | 6.3 % Show Supplier Material materials with Mangan of 6.3 % | ||
Molybdän | 1 % Show Supplier Material materials with Molybdän of 1 % | ||
Nickel | 9.5 % Show Supplier Material materials with Nickel of 9.5 % | ||
Niobium | 1 % Show Supplier Material materials with Niobium of 1 % | ||
Phosphor | 0.04 % Show Supplier Material materials with Phosphor of 0.04 % | max. | |
Schwefel | 0.015 % Show Supplier Material materials with Schwefel of 0.015 % | max. | |
Silizium | 0.5 % Show Supplier Material materials with Silizium of 0.5 % | ||
Vanadium | 0.3 % Show Supplier Material materials with Vanadium of 0.3 % |
Technological properties
Property | ||
---|---|---|
Application areas | The high creep strength of Esshete 1250, combined with its good resistance to steam and flue gas atmospheres, makes it a very suitable material for use in coal-fired boilers. The grade was developed in the United Kingdom in the 1960's, and the bulk of the material has been used in the UK power industry in 500 and 660 MW boilers. The main application has been superheaters and reheaters operating at 570°C (1058°F), steam pressure 170 bar (superheaters) and 40 bar (reheaters). Typical metal temperature 600–700°C (1112–1292°F), in flue gas temperature 900–1200°C (1652–2192°F). The corrosion environment on the fireside in the UK boilers was historically very aggressive as the British coal has, typically a high chlorine content of up to 0.6%, sulphur at 1–2% and a high ash content of 20%. Esshete 1250 has also been used successfully in superheaters in biomass boilers, burning various biofuels and producing steam at 580–540°C (1076–1004°F) at 60–200 bars pressure. Trademark information: Esshete 1250 is a trademark owned by Corus | |
Certifications | Approvals: VdTÜV-Werkstoffblatt 520 and PED (Pressure Equipment Directive) 2014/68/EU | |
Cold Forming | Esshete 1250 can be cold bent to narrow bending radii. Heat treatment after cold bending is not normally necessary, but this must be decided after considering the degree of bending and the operating conditions. If post bending heat treatment is carried out, it should be in the form of solution annealing. | |
Corrosion properties | Air: Good resistance to scaling up to 800°C (1472°F). Gaseous corrosion: Good resistance to steam and flue gas atmospheres. In service conditions typical of coal-fired boilers, the alloy has a very similar fireside corrosion to alloys of the ASTM 316H type. However, the much increased high-temperature strength gives significantly improved service performance. Fireside corrosion resistance in coal-fired, biomass-fired or coal/biomass co-fired boilers is similar to that of type ASTM 347H. Steam-side corrosion is similar to that of type ASTM 347H. | |
Heat Treatment | Tubes are delivered in the heat treated condition. If another heat treatment is needed after further processing the following is recommended: Stress relieving: 850–950°C (1560–1740°F), 10–15 minutes, cooling in air. Solution annealing: 1050–1150°C (1920–2100°F), 5–20 minutes, rapid cooling in air, gas or water. | |
Hot forming | Hot bending is carried out at 1100–850°C (1832–1652°F) and should be followed by solution annealing. | |
Other | Forms of supply: Seamless tube and pipe in Esshete 1250 is supplied in dimensions up to 260 mm (10.24 in.) outside diameter, in the solution annealed and white-pickled condition or in the bright annealed condition. | |
Structural Stability | As in other austenitic stainless steels, sigma phase can be formed after long heat treatment in the range 550–950°C (1022–1742oF). Due to the low chromium content, Esshete 1250 is significantly less sensitive to sigma phase formation than steels of e.g. the ASTM 316 type, according to tests involving ageing for 100000 h. | |
Welding | The weldability of Esshete 1250 is good. Welding must be carried out without preheating and subsequent heat treatment is normally not required. Suitable methods of fusion welding are manual metal-arc welding (MMA/SMAW) and gas-shielded arc welding, with the TIG/GTAW method as first choice. For Esshete 1250, heat input of <1.5 kJ/mm and interpass temperature of <150°C (300°F) are recommended. Recommended filler metals:
|