General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.84 g/cm³ Show Material materials with Densidad of 2.84 g/cm³ | T73 | AA Standards, ASTM B247 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||
Dureza Brinell | 135.0 [-] Show Material materials with Dureza Brinell of 135.0 [-] | T73 | AA Standards | |
Módulo de cizallamiento | 26.4 - 27.1 GPa Show Material materials with Módulo de cizallamiento of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||
Módulo elástico | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T73 | AA Standards, ASTM B247 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||
Resistencia a la tracción | 455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T73 | AA Standards, ASTM B247 | |
460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T73 | AA Standards, ASTM B247 | ||
470.0 MPa Show Material materials with Resistencia a la tracción of 470.0 MPa | T73 | AA Standards, ASTM B247 | ||
475.0 MPa Show Material materials with Resistencia a la tracción of 475.0 MPa | T73 | AA Standards, ASTM B247 | ||
485.0 MPa Show Material materials with Resistencia a la tracción of 485.0 MPa | T73 | AA Standards, ASTM B247 | ||
490.0 MPa Show Material materials with Resistencia a la tracción of 490.0 MPa | T73 | AA Standards, ASTM B247 | ||
495.0 MPa Show Material materials with Resistencia a la tracción of 495.0 MPa | T73 | AA Standards, ASTM B247 | ||
515.0 MPa Show Material materials with Resistencia a la tracción of 515.0 MPa | T73 | AA Standards |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 795.0 - 1050.0 J/(kg·K) Show Material materials with Calor específico of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium | |||
Coeficiente de dilatación térmica | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T73 | AA Standards, ASTM B247 | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T73 | AA Standards, ASTM B247 | ||
Conductividad térmica | 155 W/(m·K) Show Material materials with Conductividad térmica of 155 W/(m·K) | T73 | AA Standards, ASTM B247 | ||
Temperatura de fusión | 475.0 - 635.0 °C Show Material materials with Temperatura de fusión of 475.0 - 635.0 °C | T73 | AA Standards, ASTM B247 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 23000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 S/m | T73 | AA Standards, ASTM B247 |
Resistividad eléctrica | 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.35e-08 Ω·m | T73 | AA Standards, ASTM B247 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 1.2 - 1.9 % Show Material materials with Cobre of 1.2 - 1.9 % | T73 | AA Standards, ASTM B247 |
Cromo | 0.1 - 0.22 % Show Material materials with Cromo of 0.1 - 0.22 % | T73 | AA Standards, ASTM B247 |
Hierro | 0.35 % Show Material materials with Hierro of 0.35 % | T73 | AA Standards, ASTM B247 |
Magnesio | 2.0 - 2.9 % Show Material materials with Magnesio of 2.0 - 2.9 % | T73 | AA Standards, ASTM B247 |
Manganeso | 0.2 % Show Material materials with Manganeso of 0.2 % | T73 | AA Standards, ASTM B247 |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | T73 | AA Standards, ASTM B247 |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | T73 | AA Standards, ASTM B247 |
Zinc | 7.2 - 8.2 % Show Material materials with Zinc of 7.2 - 8.2 % | T73 | AA Standards, ASTM B247 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: good to acceptable | |
Workability | general (condition): not suitable |