General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T651 | EN 573-3 | Flat, Sheet |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Dureza Brinell | 98.0 [-] Show Material materials with Dureza Brinell of 98.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
101.0 [-] Show Material materials with Dureza Brinell of 101.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
104.0 [-] Show Material materials with Dureza Brinell of 104.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 98.0 - 104.0 [-] Show Material materials with Dureza Brinell of 98.0 - 104.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 98.0 - 101.0 [-] Show Material materials with Dureza Brinell of 98.0 - 101.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 98.0 [-] Show Material materials with Dureza Brinell of 98.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 101.0 - 104.0 [-] Show Material materials with Dureza Brinell of 101.0 - 104.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 101.0 [-] Show Material materials with Dureza Brinell of 101.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 104.0 [-] Show Material materials with Dureza Brinell of 104.0 [-] | T651 | EN 573-3 | Flat | ||
Elongación | 5.0 % Show Material materials with Elongación of 5.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | |
6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | ||
7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
8.0 % Show Material materials with Elongación of 8.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
9.0 % Show Material materials with Elongación of 9.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
10.0 % Show Material materials with Elongación of 10.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T651 | EN 573-3 | |||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3 | Sheet | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3 | Sheet | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T651 | EN 573-3 | Sheet | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T651 | EN 573-3 | Sheet, Flat | A50 | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T651 | EN 573-3 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T651 | EN 573-3 | Flat | A50 | |
Módulo de cizallamiento | 26.4 GPa Show Material materials with Módulo de cizallamiento of 26.4 GPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 25.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 27.0 GPa | T651 | EN 573-3 | Flat, Sheet | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 68.0 - 70.0 GPa Show Material materials with Módulo elástico of 68.0 - 70.0 GPa | T651 | EN 573-3 | Flat, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||||
Resistencia a la tracción | 330.0 MPa Show Material materials with Resistencia a la tracción of 330.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
340.0 MPa Show Material materials with Resistencia a la tracción of 340.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 330.0 MPa Show Material materials with Resistencia a la tracción of 330.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 330.0 MPa Show Material materials with Resistencia a la tracción of 330.0 MPa | T651 | EN 573-3 | Sheet | ||
20.0 °C | 340.0 MPa Show Material materials with Resistencia a la tracción of 340.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 340.0 MPa Show Material materials with Resistencia a la tracción of 340.0 MPa | T651 | EN 573-3 | Sheet | ||
20.0 °C | 350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | T651 | EN 573-3 | Flat | ||
Ángulo de flexión a 90° | 3.5 °/t Show Material materials with Ángulo de flexión a 90° of 3.5 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
4.0 °/t Show Material materials with Ángulo de flexión a 90° of 4.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
5.5 °/t Show Material materials with Ángulo de flexión a 90° of 5.5 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
8.0 °/t Show Material materials with Ángulo de flexión a 90° of 8.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | T651 | EN 573-3 | Flat, Sheet | |
Coeficiente de dilatación térmica | -50 °C | 2.14e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.14e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat |
-50.0 °C | 2.14e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.14e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
20 °C | 2.14e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.14e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
20 °C | 2.31e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.31e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
20 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4999999999999998e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
100 °C | 2.31e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.31e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
100.0 °C | 2.31e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.31e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
200 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
200.0 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
300 °C | 2.4999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4999999999999998e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
300.0 °C | 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5e-05 1/K | T651 | EN 573-3 | Flat, Sheet | |
Conductividad térmica | 20.0 °C | 130.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 160.0 W/(m·K) | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Temperatura de fusión | 600.0 - 650.0 °C Show Material materials with Temperatura de fusión of 600.0 - 650.0 °C | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 19000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 23000000.0 S/m | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Resistividad eléctrica | 4.35e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.35e-08 - 5.26e-08 Ω·m | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Circonio | 0.08 - 0.2 % Show Material materials with Circonio of 0.08 - 0.2 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Cobre | 0.2 % Show Material materials with Cobre of 0.2 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Cromo | 0.1 - 0.35 % Show Material materials with Cromo of 0.1 - 0.35 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | T651 | EN 573-3 | Flat, Sheet |
0.40 % Show Material materials with Hierro of 0.40 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
Magnesio | 1.0 - 1.4 % Show Material materials with Magnesio of 1.0 - 1.4 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Manganeso | 0.05 - 0.5 % Show Material materials with Manganeso of 0.05 - 0.5 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Silicona | 0.35 % Show Material materials with Silicona of 0.35 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Zinc | 4.0 - 5.0 % Show Material materials with Zinc of 4.0 - 5.0 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): good (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) good (O) / good (O) |