General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.8 g/cm³ Show Material materials with Densidad of 2.8 g/cm³ | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 140.0 MPa Show Material materials with Bending Fatigue Strength of 140.0 MPa | T4 | EN 573-3, EN 1301, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 110.0 [-] Show Material materials with Dureza Brinell of 110.0 [-] | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 110.0 [-] Show Material materials with Dureza Brinell of 110.0 [-] | T4 | EN 573-3 | Profile, Rod, Flat, Tube | ||
Elongación | 7.0 % Show Material materials with Elongación of 7.0 % | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | |
8.0 % Show Material materials with Elongación of 8.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
10.0 % Show Material materials with Elongación of 10.0 % | T4 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
10.0 % Show Material materials with Elongación of 10.0 % | T4 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
11.0 % Show Material materials with Elongación of 11.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
11.0 % Show Material materials with Elongación of 11.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
12.0 % Show Material materials with Elongación of 12.0 % | T4 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
14.0 % Show Material materials with Elongación of 14.0 % | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
18.0 % Show Material materials with Elongación of 18.0 % | T4 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T4 | EN 573-3 | Flat | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T4 | EN 573-3 | Rod | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T4 | EN 573-3 | Rod, Tube, Profile | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T4 | EN 573-3 | Rod, Flat, Profile | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | T4 | EN 573-3 | Rod | A50 | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | T4 | EN 573-3 | Tube, Profile | ||
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | T4 | EN 573-3 | Rod, Tube, Flat | ||
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3 | Flat | A50 | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3 | Rod | ||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T4 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | T4 | EN 573-3 | Wire | A100 | |
Módulo de cizallamiento | 27.4 GPa Show Material materials with Módulo de cizallamiento of 27.4 GPa | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Resistencia a la tracción | 350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
370.0 MPa Show Material materials with Resistencia a la tracción of 370.0 MPa | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
380.0 MPa Show Material materials with Resistencia a la tracción of 380.0 MPa | T4 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
390.0 MPa Show Material materials with Resistencia a la tracción of 390.0 MPa | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
20.0 °C | 350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | T4 | EN 573-3 | Rod | ||
20.0 °C | 370.0 MPa Show Material materials with Resistencia a la tracción of 370.0 MPa | T4 | EN 573-3 | Rod, Tube, Profile | ||
20.0 °C | 380.0 MPa Show Material materials with Resistencia a la tracción of 380.0 MPa | T4 | EN 573-3 | Rod, Tube, Wire | ||
20.0 °C | 390.0 MPa Show Material materials with Resistencia a la tracción of 390.0 MPa | T4 | EN 573-3 | Rod | ||
20.0 °C | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T4 | EN 573-3 | Flat | ||
20.0 °C | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T4 | EN 573-3 | Flat | ||
20.0 °C | 400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T4 | EN 573-3 | Rod, Profile | ||
Ángulo de flexión a 90° | 3.0 °/t Show Material materials with Ángulo de flexión a 90° of 3.0 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
5.0 °/t Show Material materials with Ángulo de flexión a 90° of 5.0 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 816.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Coeficiente de dilatación térmica | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Conductividad térmica | 112.0 - 251.0 W/(m·K) Show Material materials with Conductividad térmica of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Temperatura de fusión | 500.0 - 650.0 °C Show Material materials with Temperatura de fusión of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 30000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
Resistividad eléctrica | 3.4e-08 - 6e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Berilio | 0.0001 - 0.005 % Show Material materials with Berilio of 0.0001 - 0.005 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Cobre | 3.9 - 5.0 % Show Material materials with Cobre of 3.9 - 5.0 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T4 | EN 573-3 | Rod, Flat, Tube, Profile, Wire |
0.50 % Show Material materials with Hierro of 0.50 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
Magnesio | 0.2 - 0.8 % Show Material materials with Magnesio of 0.2 - 0.8 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube |
Manganeso | 0.4 - 1.2 % Show Material materials with Manganeso of 0.4 - 1.2 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube |
Níquel | 0.1 % Show Material materials with Níquel of 0.1 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube |
Silicona | 0.5 - 0.9 % Show Material materials with Silicona of 0.5 - 0.9 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T4 | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |