General
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 123.0 [-] Show Material materials with Dureza Brinell of 123.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
126.0 [-] Show Material materials with Dureza Brinell of 126.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
131.0 [-] Show Material materials with Dureza Brinell of 131.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
133.0 [-] Show Material materials with Dureza Brinell of 133.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
135.0 [-] Show Material materials with Dureza Brinell of 135.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
138.0 [-] Show Material materials with Dureza Brinell of 138.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
20.0 °C | 123.0 - 133.0 [-] Show Material materials with Dureza Brinell of 123.0 - 133.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 123.0 - 135.0 [-] Show Material materials with Dureza Brinell of 123.0 - 135.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 123.0 - 138.0 [-] Show Material materials with Dureza Brinell of 123.0 - 138.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 123.0 - 131.0 [-] Show Material materials with Dureza Brinell of 123.0 - 131.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 123.0 - 126.0 [-] Show Material materials with Dureza Brinell of 123.0 - 126.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 123.0 [-] Show Material materials with Dureza Brinell of 123.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 126.0 - 133.0 [-] Show Material materials with Dureza Brinell of 126.0 - 133.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 126.0 - 135.0 [-] Show Material materials with Dureza Brinell of 126.0 - 135.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 126.0 - 138.0 [-] Show Material materials with Dureza Brinell of 126.0 - 138.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 126.0 - 131.0 [-] Show Material materials with Dureza Brinell of 126.0 - 131.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 126.0 [-] Show Material materials with Dureza Brinell of 126.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 131.0 - 133.0 [-] Show Material materials with Dureza Brinell of 131.0 - 133.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 131.0 - 135.0 [-] Show Material materials with Dureza Brinell of 131.0 - 135.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 131.0 - 138.0 [-] Show Material materials with Dureza Brinell of 131.0 - 138.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 131.0 [-] Show Material materials with Dureza Brinell of 131.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 133.0 [-] Show Material materials with Dureza Brinell of 133.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 133.0 - 135.0 [-] Show Material materials with Dureza Brinell of 133.0 - 135.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 133.0 - 138.0 [-] Show Material materials with Dureza Brinell of 133.0 - 138.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 135.0 [-] Show Material materials with Dureza Brinell of 135.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 135.0 - 138.0 [-] Show Material materials with Dureza Brinell of 135.0 - 138.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 138.0 [-] Show Material materials with Dureza Brinell of 138.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 140.0 [-] Show Material materials with Dureza Brinell of 140.0 [-] | T651 | EN 573-3 | Rod | ||
20.0 °C | 150.0 [-] Show Material materials with Dureza Brinell of 150.0 [-] | T651 | EN 573-3 | Flat | ||
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | |
4.0 % Show Material materials with Elongación of 4.0 % | T651 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
4.0 % Show Material materials with Elongación of 4.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
5.0 % Show Material materials with Elongación of 5.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | T651 | EN 573-3 | Sheet | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T651 | EN 573-3 | Rod | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T651 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T651 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T651 | EN 573-3 | Rod, Flat | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T651 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T651 | EN 573-3 | Flat | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T651 | EN 573-3 | Transverse | ||
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T651 | EN 573-3 | Sheet | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | T651 | EN 573-3 | A50 Transverse | ||
Límite elástico | -196.0 °C | 432.0 MPa Show Material materials with Límite elástico of 432.0 MPa | T651 | EN 573-3 | ||
340.0 MPa Show Material materials with Límite elástico of 340.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
350.0 MPa Show Material materials with Límite elástico of 350.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
360.0 MPa Show Material materials with Límite elástico of 360.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
380.0 MPa Show Material materials with Límite elástico of 380.0 MPa | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
390.0 MPa Show Material materials with Límite elástico of 390.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
395.0 MPa Show Material materials with Límite elástico of 395.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
400.0 MPa Show Material materials with Límite elástico of 400.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | RP02 | ||
20.0 °C | 140.0 - 250.0 MPa Show Material materials with Límite elástico of 140.0 - 250.0 MPa | T651 | EN 573-3 | RP02 Transverse | ||
20.0 °C | 240.0 MPa Show Material materials with Límite elástico of 240.0 MPa | T651 | EN 573-3 | Sheet | RP02 Transverse | |
20.0 °C | 340.0 MPa Show Material materials with Límite elástico of 340.0 MPa | T651 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 340.0 MPa Show Material materials with Límite elástico of 340.0 MPa | T651 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 350.0 MPa Show Material materials with Límite elástico of 350.0 MPa | T651 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 350.0 MPa Show Material materials with Límite elástico of 350.0 MPa | T651 | EN 573-3 | Sheet, Flat | RP02 | |
20.0 °C | 360.0 MPa Show Material materials with Límite elástico of 360.0 MPa | T651 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 360.0 MPa Show Material materials with Límite elástico of 360.0 MPa | T651 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 370.0 MPa Show Material materials with Límite elástico of 370.0 MPa | T651 | EN 573-3 | Flat | RP02 | |
20.0 °C | 380.0 MPa Show Material materials with Límite elástico of 380.0 MPa | T651 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 380.0 MPa Show Material materials with Límite elástico of 380.0 MPa | T651 | EN 573-3 | Rod, Sheet, Flat | RP02 | |
20.0 °C | 390.0 MPa Show Material materials with Límite elástico of 390.0 MPa | T651 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 390.0 MPa Show Material materials with Límite elástico of 390.0 MPa | T651 | EN 573-3 | Sheet, Flat | RP02 | |
20.0 °C | 395.0 MPa Show Material materials with Límite elástico of 395.0 MPa | T651 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 395.0 MPa Show Material materials with Límite elástico of 395.0 MPa | T651 | EN 573-3 | Flat | RP02 | |
20.0 °C | 400.0 MPa Show Material materials with Límite elástico of 400.0 MPa | T651 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 400.0 MPa Show Material materials with Límite elástico of 400.0 MPa | T651 | EN 573-3 | Flat | RP02 | |
20.0 °C | 410.0 MPa Show Material materials with Límite elástico of 410.0 MPa | T651 | EN 573-3 | Flat | RP02 | |
20.0 °C | 432.0 MPa Show Material materials with Límite elástico of 432.0 MPa | T651 | EN 573-3 | |||
20.0 °C | 440.0 MPa Show Material materials with Límite elástico of 440.0 MPa | T651 | EN 573-3 | Sheet | ||
Módulo de cizallamiento | 27.4 GPa Show Material materials with Módulo de cizallamiento of 27.4 GPa | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20.0 °C | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T651 | EN 573-3 | Rod, Sheet, Flat | ||
Plane-Strain Fracture Toughnes | -196.0 °C | 28.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.5 MPa·√m | T651 | EN 573-3 | ||
20.0 °C | 19.0 - 24.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.0 - 24.0 MPa·√m | T651 | EN 573-3 | Sheet | ||
20.0 °C | 19.0 - 22.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.0 - 22.0 MPa·√m | T651 | EN 573-3 | Sheet | ||
20.0 °C | 19.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.0 MPa·√m | T651 | EN 573-3 | Sheet | ||
20.0 °C | 19.5 - 25.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.5 - 25.5 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 19.5 - 23.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.5 - 23.5 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 19.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.5 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 19.5 - 23.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.5 - 23.2 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 22.0 - 24.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 24.0 MPa·√m | T651 | EN 573-3 | Sheet | ||
20.0 °C | 22.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 MPa·√m | T651 | EN 573-3 | Sheet | ||
20.0 °C | 23.2 - 25.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 23.2 - 25.5 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 23.2 - 23.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 23.2 - 23.5 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 23.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 23.2 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 23.5 - 25.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 23.5 - 25.5 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 23.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 23.5 MPa·√m | T651 | EN 573-3 | |||
20.0 °C | 24.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 MPa·√m | T651 | EN 573-3 | Sheet | ||
20.0 °C | 25.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 MPa·√m | T651 | EN 573-3 | |||
Resistencia a la tracción | 390.0 MPa Show Material materials with Resistencia a la tracción of 390.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
20.0 °C | 220.0 - 400.0 MPa Show Material materials with Resistencia a la tracción of 220.0 - 400.0 MPa | T651 | EN 573-3 | Transverse | ||
20.0 °C | 390.0 MPa Show Material materials with Resistencia a la tracción of 390.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 390.0 MPa Show Material materials with Resistencia a la tracción of 390.0 MPa | T651 | EN 573-3 | Sheet | ||
20.0 °C | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T651 | EN 573-3 | Sheet | Transverse | |
20.0 °C | 410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T651 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T651 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 430.0 MPa Show Material materials with Resistencia a la tracción of 430.0 MPa | T651 | EN 573-3 | Flat | ||
20.0 °C | 435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T651 | EN 573-3 | Sheet | ||
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T651 | EN 573-3 | Flat | ||
20.0 °C | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T651 | EN 573-3 | Rod, Sheet, Flat | ||
20.0 °C | 460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T651 | EN 573-3 | Flat | ||
Ángulo de flexión a 90° | 5.0 °/t Show Material materials with Ángulo de flexión a 90° of 5.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
7.0 °/t Show Material materials with Ángulo de flexión a 90° of 7.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
10.0 °/t Show Material materials with Ángulo de flexión a 90° of 10.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 816.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | ||||
Coeficiente de dilatación térmica | -50 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | |
-50.0 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
20 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
20 °C | 2.28e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.28e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
20 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
20 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
100 °C | 2.28e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.28e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
100.0 °C | 2.28e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.28e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
100 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
200 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
200.0 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
300 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
300.0 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar, Rod, Flat | ||
Conductividad térmica | 134.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 134.0 - 193.0 W/(m·K) | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20.0 °C | 140.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 - 200.0 W/(m·K) | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar | ||
Temperatura de fusión | 505.0 - 635.0 °C Show Material materials with Temperatura de fusión of 505.0 - 635.0 °C | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
510.0 - 640.0 °C Show Material materials with Temperatura de fusión of 510.0 - 640.0 °C | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 21000000.0 - 24000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 - 24000000.0 S/m | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | |
20.0 °C | 20000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 29000000.0 S/m | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar | |
Resistividad eléctrica | 3.45e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 5e-08 Ω·m | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | |
4.17e-08 - 4.76e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.17e-08 - 4.76e-08 Ω·m | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 3.9 - 5.0 % Show Material materials with Cobre of 3.9 - 5.0 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T651 | EN 573-3 | Flat |
0.7 % Show Material materials with Hierro of 0.7 % | T651 | EN 573-3 | Rod, Sheet, Flat | |
0.70 % Show Material materials with Hierro of 0.70 % | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | |
Magnesio | 0.2 - 0.8 % Show Material materials with Magnesio of 0.2 - 0.8 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar |
Manganeso | 0.4 - 1.2 % Show Material materials with Manganeso of 0.4 - 1.2 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar |
Níquel | 0.1 Show Material materials with Níquel of 0.1 | T651 | EN 573-3 | Flat |
Silicona | 0.5 - 1.2 % Show Material materials with Silicona of 0.5 - 1.2 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar |
0.5 - 0.9 % Show Material materials with Silicona of 0.5 - 0.9 % | T651 | EN 573-3 | Flat | |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable |