General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Elongación | 4.0 % Show Material materials with Elongación of 4.0 % | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | |
5.0 % Show Material materials with Elongación of 5.0 % | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T851 | EN 573-3 | Sheet | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T851 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T851 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T851 | EN 573-3 | Flat | A50 | |
Módulo de cizallamiento | 26.0 - 27.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Módulo elástico | 70.0 - 73.0 GPa Show Material materials with Módulo elástico of 70.0 - 73.0 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Resistencia a la tracción | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
405.0 MPa Show Material materials with Resistencia a la tracción of 405.0 MPa | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
20.0 °C | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T851 | EN 573-3 | Sheet | ||
20.0 °C | 405.0 MPa Show Material materials with Resistencia a la tracción of 405.0 MPa | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 405.0 MPa Show Material materials with Resistencia a la tracción of 405.0 MPa | T851 | EN 573-3 | Sheet | ||
20.0 °C | 410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T851 | EN 573-3 | Sheet | ||
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T851 | EN 573-3 | Flat |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 816.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Coeficiente de dilatación térmica | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Conductividad térmica | 112.0 - 251.0 W/(m·K) Show Material materials with Conductividad térmica of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Temperatura de fusión | 500.0 - 650.0 °C Show Material materials with Temperatura de fusión of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 30000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
Resistividad eléctrica | 3.4e-08 - 6e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 1.8 - 2.7 % Show Material materials with Cobre of 1.8 - 2.7 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Hierro | 0.9 - 1.4 % Show Material materials with Hierro of 0.9 - 1.4 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Magnesio | 1.2 - 1.8 % Show Material materials with Magnesio of 1.2 - 1.8 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Manganeso | 0.25 % Show Material materials with Manganeso of 0.25 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Níquel | 0.8 - 1.4 % Show Material materials with Níquel of 0.8 - 1.4 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Silicona | 0.15 - 0.25 % Show Material materials with Silicona of 0.15 - 0.25 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Zinc | 0.15 % Show Material materials with Zinc of 0.15 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |