General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Dureza Brinell (HBW) | 27 [-] Show Material materials with Dureza Brinell (HBW) of 27 [-] | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | ||
Elongación | 1 % Show Material materials with Elongación of 1 % | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Sheet | A50 | |
20.0 °C | 22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3 | Tube | ||
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3 | Sheet | A50 | |
Límite elástico | 35 MPa Show Material materials with Límite elástico of 35 MPa | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | ||
20.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Tube, Sheet | RP02 | |
Módulo de cizallamiento | 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 90 MPa Show Material materials with Resistencia a la tracción of 90 MPa | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | ||
20.0 °C | 90.0 MPa Show Material materials with Resistencia a la tracción of 90.0 MPa | O | EN 573-3 | Sheet | ||
20.0 °C | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | O | EN 573-3 | Tube | ||
20.0 °C | 100.0 MPa Show Material materials with Resistencia a la tracción of 100.0 MPa | O | EN 573-3 | Sheet | ||
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | ||
Ángulo de flexión a 90° | 0 °/t Show Material materials with Ángulo de flexión a 90° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 - 920.0 J/(kg·K) Show Material materials with Calor específico of 893.0 - 920.0 J/(kg·K) | Typical for Wrought 3000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 100 °C | 0.000023 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000023 1/K | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | 20-100°C |
Conductividad térmica | 176 W/(m·K) Show Material materials with Conductividad térmica of 176 W/(m·K) | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | ||
Temperatura de fusión | 629.0 - 654.0 °C Show Material materials with Temperatura de fusión of 629.0 - 654.0 °C | Typical for Wrought 3000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 29000000.0 S/m | Typical for Wrought 3000 Series Aluminium | |||
Resistividad eléctrica | 4.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-3 | Sheet, Tube |
0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | O | EN 573-3 | Sheet, Tube |
0.1 % Show Material materials with Cromo of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-3 | Sheet, Tube |
0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | |
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | O | EN 573-3 | Sheet, Tube |
0.3 % Show Material materials with Magnesio of 0.3 % | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | |
Manganeso | 0.7 - 1.4 % Show Material materials with Manganeso of 0.7 - 1.4 % | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3 | Sheet, Tube, Coil, Sheet |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | O | EN 573-3 | Sheet, Tube |
0.5 % Show Material materials with Silicona of 0.5 % | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet | |
Titanio | 0.1 Show Material materials with Titanio of 0.1 | O | EN 573-3 | Sheet, Tube |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | O | EN 573-3 | Sheet, Tube |
0.2 % Show Material materials with Zinc of 0.2 % | O | EN 573-1, EN 573-2, EN 573-3 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | Very Good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Heat exchangers: Fins, Heat exchangers; Tubes: Flexible tube, Pipes; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Components: Automotive fins, Heat exchangers | |
Brazing | Excellent | |
Corrosion properties | Very Good | |
Welding | Very Good | |
Workability | Very Good |