General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H112 | EN 573-3 | Profile, Rod, Flat, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
Dureza Brinell | 28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
34.0 [-] Show Material materials with Dureza Brinell of 34.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | H112 | EN 573-3 | Profile, Rod, Tube, Flat | ||
20.0 °C | 28.0 - 34.0 [-] Show Material materials with Dureza Brinell of 28.0 - 34.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 34.0 [-] Show Material materials with Dureza Brinell of 34.0 [-] | H112 | EN 573-3 | Flat | ||
Elongación | 10.0 % Show Material materials with Elongación of 10.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
17.0 % Show Material materials with Elongación of 17.0 % | H112 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
18.0 % Show Material materials with Elongación of 18.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 % Show Material materials with Elongación of 20.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
25.0 % Show Material materials with Elongación of 25.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H112 | EN 573-3 | Flat | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H112 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | H112 | EN 573-3 | Tube | ||
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | H112 | EN 573-3 | Flat | ||
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | H112 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | H112 | EN 573-3 | Profile, Rod, Tube | ||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.1 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.1 - 26.5 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
Módulo elástico | -270 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | |
-270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | ||
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Módulo elástico of 69.0 - 69.5 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Módulo elástico of 69.5 - 70.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
20 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube | ||
300 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
110.0 MPa Show Material materials with Resistencia a la tracción of 110.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | H112 | EN 573-3 | Profile, Rod, Tube, Flat | ||
20.0 °C | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 110.0 MPa Show Material materials with Resistencia a la tracción of 110.0 MPa | H112 | EN 573-3 | Flat | ||
20.0 °C | 110.0 MPa Show Material materials with Resistencia a la tracción of 110.0 MPa | H112 | EN 573-3 | Flat | Transverse |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Calor específico of 892.0 - 893.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 892.0 J/(kg·K) Show Material materials with Calor específico of 892.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Conductividad térmica | 20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat |
20.0 °C | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 28000000.0 S/m | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 29000000.0 S/m | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
Resistividad eléctrica | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.57e-08 - 4.55e-08 Ω·m | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.1e-08 Ω·m | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.5e-08 Ω·m | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 Ω·m | H112 | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 - 4.5e-08 Ω·m | H112 | EN 573-3 | Profile, Rod, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H112 | EN 573-3 | Profile, Rod, Flat, Tube |
0.70 % Show Material materials with Hierro of 0.70 % | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |