General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Foil, Rod, Sheet, Flat, Tube, Wire, Coil, Sheet |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 50.0 MPa Show Material materials with Bending Fatigue Strength of 50.0 MPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | |
Dureza Brinell | 27.0 [-] Show Material materials with Dureza Brinell of 27.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 27.0 [-] Show Material materials with Dureza Brinell of 27.0 [-] | O | EN 573-3 | Flat | ||
20.0 °C | 28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 29.0 [-] Show Material materials with Dureza Brinell of 29.0 [-] | O | EN 573-3 | Rod, Tube | ||
Dureza Brinell (HBW) | 27 [-] Show Material materials with Dureza Brinell (HBW) of 27 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
Elongación | -196.0 °C | 46.0 % Show Material materials with Elongación of 46.0 % | O | EN 573-3 | ||
-80.0 °C | 42.0 % Show Material materials with Elongación of 42.0 % | O | EN 573-3 | |||
-20.0 °C | 41.0 % Show Material materials with Elongación of 41.0 % | O | EN 573-3 | |||
7.0 % Show Material materials with Elongación of 7.0 % | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
17.0 - 21.0 % Show Material materials with Elongación of 17.0 - 21.0 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | A50 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
21.0 % Show Material materials with Elongación of 21.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
25.0 % Show Material materials with Elongación of 25.0 % | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
28.0 % Show Material materials with Elongación of 28.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Foil, Sheet | A50 | |
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 21.0 % Show Material materials with Elongación of 21.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 21.0 % Show Material materials with Elongación of 21.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3 | Tube | ||
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3 | Sheet | A50 | |
20.0 °C | 24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | O | EN 573-3 | Rod, Tube, Flat | ||
20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 28.0 % Show Material materials with Elongación of 28.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 28.0 % Show Material materials with Elongación of 28.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3 | Wire | A100 | |
20.0 °C | 40.0 % Show Material materials with Elongación of 40.0 % | O | EN 573-3 | |||
100.0 °C | 43.0 % Show Material materials with Elongación of 43.0 % | O | EN 573-3 | |||
150.0 °C | 47.0 % Show Material materials with Elongación of 47.0 % | O | EN 573-3 | |||
200.0 °C | 60.0 % Show Material materials with Elongación of 60.0 % | O | EN 573-3 | |||
260.0 °C | 65.0 % Show Material materials with Elongación of 65.0 % | O | EN 573-3 | |||
320.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | O | EN 573-3 | |||
370.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | O | EN 573-3 | |||
Límite elástico | -270 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat | RP02 |
-270.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat | RP02 | |
-196.0 °C | 60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3 | Wire | RP02 | |
-80.0 °C | 49.0 MPa Show Material materials with Límite elástico of 49.0 MPa | O | EN 573-3 | RP02 | ||
-20.0 °C | 46.0 MPa Show Material materials with Límite elástico of 46.0 MPa | O | EN 573-3 | RP02 | ||
35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
35 MPa Show Material materials with Límite elástico of 35 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
20.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat | RP02 | |
20 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat | RP02 | |
20.0 °C | 35.0 - 42.0 MPa Show Material materials with Límite elástico of 35.0 - 42.0 MPa | O | EN 573-3 | RP02 | ||
20.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 42.0 MPa Show Material materials with Límite elástico of 42.0 MPa | O | EN 573-3 | RP02 | ||
20.0 °C | 60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3 | Wire | RP02 | |
20.0 °C | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | O | EN 573-3 | Foil | RP02 | |
50 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat | RP02 | |
50.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat | RP02 | |
100.0 °C | 37.0 MPa Show Material materials with Límite elástico of 37.0 MPa | O | EN 573-3 | RP02 | ||
150.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat | RP02 | |
200.0 °C | 30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | O | EN 573-3 | RP02 | ||
260.0 °C | 24.0 MPa Show Material materials with Límite elástico of 24.0 MPa | O | EN 573-3 | RP02 | ||
320.0 °C | 17.0 MPa Show Material materials with Límite elástico of 17.0 MPa | O | EN 573-3 | RP02 | ||
370.0 °C | 12.0 MPa Show Material materials with Límite elástico of 12.0 MPa | O | EN 573-3 | RP02 | ||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.1 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.1 - 26.5 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
Módulo elástico | -270 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire, Coil, Sheet | |
-270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire, Coil, Sheet | ||
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Módulo elástico of 69.0 - 69.5 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Módulo elástico of 69.5 - 70.0 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire, Coil, Sheet | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire, Coil, Sheet | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
300 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | -196.0 °C | 232.0 MPa Show Material materials with Resistencia a la tracción of 232.0 MPa | O | EN 573-3 | ||
-80.0 °C | 137.0 MPa Show Material materials with Resistencia a la tracción of 137.0 MPa | O | EN 573-3 | |||
-20.0 °C | 119.0 MPa Show Material materials with Resistencia a la tracción of 119.0 MPa | O | EN 573-3 | |||
90.0 MPa Show Material materials with Resistencia a la tracción of 90.0 MPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 80.0 - 130.0 MPa Show Material materials with Resistencia a la tracción of 80.0 - 130.0 MPa | O | EN 573-3, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 90.0 - 130.0 MPa Show Material materials with Resistencia a la tracción of 90.0 - 130.0 MPa | O | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Coil, Sheet | ||
20.0 °C | 90.0 MPa Show Material materials with Resistencia a la tracción of 90.0 MPa | O | EN 573-3 | Sheet | ||
20.0 °C | 90.0 - 130.0 MPa Show Material materials with Resistencia a la tracción of 90.0 - 130.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 95.0 - 130.0 MPa Show Material materials with Resistencia a la tracción of 95.0 - 130.0 MPa | O | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 95.0 - 135.0 MPa Show Material materials with Resistencia a la tracción of 95.0 - 135.0 MPa | O | EN 573-3, EN 755 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | O | EN 573-3 | Tube | ||
20.0 °C | 112.0 MPa Show Material materials with Resistencia a la tracción of 112.0 MPa | O | EN 573-3 | |||
20.0 °C | 130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | O | EN 573-3 | Wire | ||
100.0 °C | 91.0 MPa Show Material materials with Resistencia a la tracción of 91.0 MPa | O | EN 573-3 | |||
150.0 °C | 77.0 MPa Show Material materials with Resistencia a la tracción of 77.0 MPa | O | EN 573-3 | |||
200.0 °C | 57.0 MPa Show Material materials with Resistencia a la tracción of 57.0 MPa | O | EN 573-3 | |||
260.0 °C | 47.0 MPa Show Material materials with Resistencia a la tracción of 47.0 MPa | O | EN 573-3 | |||
320.0 °C | 28.0 MPa Show Material materials with Resistencia a la tracción of 28.0 MPa | O | EN 573-3 | |||
370.0 °C | 19.0 MPa Show Material materials with Resistencia a la tracción of 19.0 MPa | O | EN 573-3 | |||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Ángulo de flexión a 90° | 1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Calor específico of 892.0 - 893.0 J/(kg·K) | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 892.0 J/(kg·K) Show Material materials with Calor específico of 892.0 J/(kg·K) | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
100 °C | 0.000025 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000025 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | 20-100°C | |
Conductividad térmica | 176 W/(m·K) Show Material materials with Conductividad térmica of 176 W/(m·K) | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
20.0 °C | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | ||
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 28000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 29000000.0 S/m | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | |
Resistividad eléctrica | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.57e-08 - 4.55e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
4.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.1e-08 Ω·m | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.5e-08 Ω·m | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 Ω·m | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 - 4.5e-08 Ω·m | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar |
0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar |
0.1 % Show Material materials with Cromo of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-3 | Foil, Rod, Sheet, Flat, Tube, Wire |
0.70 % Show Material materials with Hierro of 0.70 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar |
0.3 % Show Material materials with Magnesio of 0.3 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar, Coil, Sheet |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar |
0.5 % Show Material materials with Silicona of 0.5 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar |
0.2 % Show Material materials with Zinc of 0.2 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Lithography; Heat exchangers: Fins, Heat exchangers; Tubes: Flexible tube, Pipes; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Components: Automotive fins, Heat exchangers | |
Brazing | hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |