General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 | ||
20.0 °C | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | O | EN 573-3, EN 1592, EN 485, EN 754, EN 755 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 69.0 [-] Show Material materials with Dureza Brinell of 69.0 [-] | O | EN 573-3, EN 485 | |||
70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | O | EN 573-3, EN 485 | ||||
73.0 [-] Show Material materials with Dureza Brinell of 73.0 [-] | O | EN 573-3, EN 485 | ||||
75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | O | EN 573-3, EN 485 | ||||
20.0 °C | 60.0 [-] Show Material materials with Dureza Brinell of 60.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod, Tube | ||
20.0 °C | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Sheet, Strip | ||
Elongación | 9.0 % Show Material materials with Elongación of 9.0 % | O | EN 573-3, EN 485 | A100 | ||
10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3, EN 485 | A100 | |||
10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3, EN 755 | A50 | |||
11.0 % Show Material materials with Elongación of 11.0 % | O | EN 573-3, EN 485 | A50 | |||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 485, EN 755 | A100 | |||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 485 | A50 | |||
13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3, EN 485 | A50 | |||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 485 | A100 | |||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 754 | A50 | |||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 485 | A100 | |||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 485 | A50 | |||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 1592, EN 754 | A100 | |||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 485 | A50 | |||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 14286 | A100 | |||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod | A10 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod | ||
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Tube | A10 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Tube, Sheet | ||
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Sheet, Strip | A10 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Sheet, Strip | ||
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
100.0 °C | 26.0 % Show Material materials with Elongación of 26.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
180.0 °C | 43.0 % Show Material materials with Elongación of 43.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
240.0 °C | 48.0 % Show Material materials with Elongación of 48.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
300.0 °C | 67.0 % Show Material materials with Elongación of 67.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
Estricción | 20.0 °C | 15.0 % Show Material materials with Estricción of 15.0 % | O | DIN 1725-1 | Sheet | |
Módulo de cizallamiento | 26.8 GPa Show Material materials with Módulo de cizallamiento of 26.8 GPa | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
20.0 °C | 27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
Módulo elástico | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
20.0 °C | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | -193.0 °C | 495.0 MPa Show Material materials with Resistencia a la tracción of 495.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | ||
-150.0 °C | 415.0 MPa Show Material materials with Resistencia a la tracción of 415.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
-105.0 °C | 370.0 MPa Show Material materials with Resistencia a la tracción of 370.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
-60.0 °C | 355.0 MPa Show Material materials with Resistencia a la tracción of 355.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
-15.0 °C | 350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
245.0 MPa Show Material materials with Resistencia a la tracción of 245.0 MPa | O | EN 573-3, EN 485 | ||||
250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | O | EN 573-3, EN 485 | ||||
255.0 MPa Show Material materials with Resistencia a la tracción of 255.0 MPa | O | EN 573-3, EN 485 | ||||
260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | O | EN 573-3, EN 485 | ||||
270.0 - 345.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 345.0 MPa | O | EN 573-3, EN 485 | ||||
270.0 - 350.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 350.0 MPa | O | EN 573-3, EN 754 | ||||
270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | O | EN 573-3, EN 755 | ||||
275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | O | EN 573-3, EN 1592 | ||||
290.0 - 370.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 370.0 MPa | O | EN 573-3, EN 14286 | ||||
20.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | O | DIN 1725-1 | Sheet | ||
20.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod, Tube | ||
20.0 °C | 275.0 - 350.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 350.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485 | Sheet, Strip | ||
20.0 °C | 321.0 MPa Show Material materials with Resistencia a la tracción of 321.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
20.0 °C | 350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
100.0 °C | 302.0 MPa Show Material materials with Resistencia a la tracción of 302.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
180.0 °C | 209.0 MPa Show Material materials with Resistencia a la tracción of 209.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
240.0 °C | 168.0 MPa Show Material materials with Resistencia a la tracción of 168.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
300.0 °C | 122.0 MPa Show Material materials with Resistencia a la tracción of 122.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | |||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | |||
1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | O | EN 573-3, EN 14286, EN 485 | ||||
4.0 °/t Show Material materials with Ángulo de flexión a 180° of 4.0 °/t | O | EN 573-3, EN 14286 | ||||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | O | EN 573-3, EN 485 | ||||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | O | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
Coeficiente de dilatación térmica | -50 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | |
-50.0 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
20 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
20 °C | 2.42e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.42e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4999999999999998e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
20 °C | 2.6e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.6e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
100 °C | 2.42e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.42e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
100.0 °C | 2.42e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.42e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
200 °C | 2.4999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4999999999999998e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
200.0 °C | 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5e-05 1/K | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
300 °C | 2.6e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.6e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
300.0 °C | 2.6e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.6e-05 1/K | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Rod, Sheet, Strip, Tube | ||
Conductividad térmica | 20.0 °C | 110.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 - 140.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube | |
Temperatura de fusión | 574.0 - 638.0 °C Show Material materials with Temperatura de fusión of 574.0 - 638.0 °C | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 | |||
Temperatura máx. de funcionamiento | -195.0 - 50.0 °C Show Material materials with Temperatura máx. de funcionamiento of -195.0 - 50.0 °C | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube | Long | |
150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 16000000.0 - 19000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 19000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube |
Resistividad eléctrica | 5.26e-08 - 6.25e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.26e-08 - 6.25e-08 Ω·m | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Sheet, Rod, Strip, Tube |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Sheet, Rod, Strip, Tube |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Sheet, Rod, Strip, Tube |
0.40 % Show Material materials with Hierro of 0.40 % | O | EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755 | ||
Magnesio | 4.0 - 4.9 % Show Material materials with Magnesio of 4.0 - 4.9 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Sheet, Rod, Strip, Tube |
Manganeso | 0.3 - 1.0 % Show Material materials with Manganeso of 0.3 - 1.0 % | O | DIN 1725-1 | Sheet |
0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube | |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Sheet, Rod, Strip, Tube |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Sheet, Rod, Strip, Tube |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Sheet, Rod, Strip, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |