General
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 145.0 MPa Show Material materials with Bending Fatigue Strength of 145.0 MPa | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 123.0 [-] Show Material materials with Dureza Brinell of 123.0 [-] | T6 | EN 573-3, EN 485 | |||
125.0 [-] Show Material materials with Dureza Brinell of 125.0 [-] | T6 | EN 573-3, EN 586 | ||||
126.0 [-] Show Material materials with Dureza Brinell of 126.0 [-] | T6 | EN 573-3, EN 485 | ||||
131.0 [-] Show Material materials with Dureza Brinell of 131.0 [-] | T6 | EN 573-3, EN 485 | ||||
133.0 [-] Show Material materials with Dureza Brinell of 133.0 [-] | T6 | EN 573-3, EN 485 | ||||
135.0 [-] Show Material materials with Dureza Brinell of 135.0 [-] | T6 | EN 573-3, EN 485 | ||||
138.0 [-] Show Material materials with Dureza Brinell of 138.0 [-] | T6 | EN 573-3, EN 485 | ||||
20.0 °C | 120.0 [-] Show Material materials with Dureza Brinell of 120.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | T6 | EN 573-3, EN 485 | A100 | ||
3.0 % Show Material materials with Elongación of 3.0 % | T6 | EN 573-3, EN 586 | A100 | |||
4.0 % Show Material materials with Elongación of 4.0 % | T6 | EN 573-3, EN 485 | A100 | |||
4.0 % Show Material materials with Elongación of 4.0 % | T6 | EN 573-3, EN 755 | A50 | |||
5.0 % Show Material materials with Elongación of 5.0 % | T6 | EN 573-3, EN 485, EN 755 | A100 | |||
5.0 % Show Material materials with Elongación of 5.0 % | T6 | EN 573-3, EN 755 | A50 | |||
6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3, EN 485, EN 755 | A100 | |||
6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3, EN 485, EN 754 | A50 | |||
7.0 % Show Material materials with Elongación of 7.0 % | T6 | EN 573-3, EN 755 | A100 | |||
7.0 % Show Material materials with Elongación of 7.0 % | T6 | EN 573-3, EN 485 | A50 | |||
8.0 % Show Material materials with Elongación of 8.0 % | T6 | EN 573-3, EN 754 | A100 | |||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
Módulo de cizallamiento | 27.4 GPa Show Material materials with Módulo de cizallamiento of 27.4 GPa | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | |||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | |||
20.0 °C | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Resistencia a la tracción | 390.0 MPa Show Material materials with Resistencia a la tracción of 390.0 MPa | T6 | EN 573-3, EN 485 | |||
410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T6 | EN 573-3, EN 485 | ||||
415.0 MPa Show Material materials with Resistencia a la tracción of 415.0 MPa | T6 | EN 573-3, EN 755 | ||||
420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T6 | EN 573-3, EN 485, EN 755 | ||||
430.0 MPa Show Material materials with Resistencia a la tracción of 430.0 MPa | T6 | EN 573-3, EN 586, EN 755 | ||||
435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T6 | EN 573-3, EN 485 | ||||
440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T6 | EN 573-3, EN 485 | ||||
450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T6 | EN 573-3, EN 485, EN 754, EN 755 | ||||
460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T6 | EN 573-3, EN 485, EN 755 | ||||
465.0 MPa Show Material materials with Resistencia a la tracción of 465.0 MPa | T6 | EN 573-3, EN 755 | ||||
20.0 °C | 400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 430.0 MPa Show Material materials with Resistencia a la tracción of 430.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
Ángulo de flexión a 90° | 5.0 °/t Show Material materials with Ángulo de flexión a 90° of 5.0 °/t | T6 | EN 573-3, EN 485 | |||
7.0 °/t Show Material materials with Ángulo de flexión a 90° of 7.0 °/t | T6 | EN 573-3, EN 485 | ||||
10.0 °/t Show Material materials with Ángulo de flexión a 90° of 10.0 °/t | T6 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 816.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | ||||
Coeficiente de dilatación térmica | -50 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | |
-50.0 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
20 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
20 °C | 2.28e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.28e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
20 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | |||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
20 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
100 °C | 2.28e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.28e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
100.0 °C | 2.28e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.28e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
100 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | |||
200 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
200.0 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
300 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
300.0 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755, DIN 1725-1, EN 573-4 | Forging | ||
Conductividad térmica | 134.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 134.0 - 193.0 W/(m·K) | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | |||
20.0 °C | 140.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 - 200.0 W/(m·K) | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging | ||
Temperatura de fusión | 505.0 - 635.0 °C Show Material materials with Temperatura de fusión of 505.0 - 635.0 °C | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | |||
510.0 - 640.0 °C Show Material materials with Temperatura de fusión of 510.0 - 640.0 °C | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 21000000.0 - 24000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 - 24000000.0 S/m | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | ||
20.0 °C | 20000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 29000000.0 S/m | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging | |
Resistividad eléctrica | 3.45e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 5e-08 Ω·m | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | ||
4.17e-08 - 4.76e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.17e-08 - 4.76e-08 Ω·m | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 3.9 - 5.0 % Show Material materials with Cobre of 3.9 - 5.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Forging |
0.70 % Show Material materials with Hierro of 0.70 % | T6 | EN 573-3, EN 485, EN 586, EN 754, EN 755 | ||
Magnesio | 0.2 - 0.8 % Show Material materials with Magnesio of 0.2 - 0.8 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging |
Manganeso | 0.4 - 1.2 % Show Material materials with Manganeso of 0.4 - 1.2 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging |
Silicona | 0.5 - 1.2 % Show Material materials with Silicona of 0.5 - 1.2 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 586, EN 754, EN 755 | Forging |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable |