General
Property | Value | Testing Standard | Condition |
---|---|---|---|
Absorción de agua | 1.9 % Show Supplier Material materials with Absorción de agua of 1.9 % | Sim. to ISO 62 | |
Densidad | 1.27 g/cm³ Show Supplier Material materials with Densidad of 1.27 g/cm³ | ISO 1183 | dry |
Moisture absorption | 0.9 % Show Supplier Material materials with Moisture absorption of 0.9 % | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Dureza Shore D | 79 [-] Show Supplier Material materials with Dureza Shore D of 79 [-] | dry | ISO 7619-1 | 15 seconds | |
Elongación | 3 % Show Supplier Material materials with Elongación of 3 % | cond., dry | ISO 527-1/-2 | ||
Módulo elástico | 8.5 GPa Show Supplier Material materials with Módulo elástico of 8.5 GPa | cond. | ISO 527-1/-2 | ||
8.9 GPa Show Supplier Material materials with Módulo elástico of 8.9 GPa | dry | ISO 527-1/-2 | |||
Resistencia a la tracción | 125 MPa Show Supplier Material materials with Resistencia a la tracción of 125 MPa | cond. | ISO 527-1/-2 | ||
130 MPa Show Supplier Material materials with Resistencia a la tracción of 130 MPa | dry | ISO 527-1/-2 | |||
Resistencia al choque, ensayo Charpy entallado | 23 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | dry | ISO 179/1eA | |
23 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | cond. | ISO 179/1eA | ||
Resistencia al choque, ensayo Charpy no entallado | No Break at 23°C | cond. | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment | ||||
---|---|---|---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1.8e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.8e-05 1/K | dry | ISO 11359-1/-2 | ||||||
0.00011 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.00011 1/K | dry | ISO 11359-1/-2 | Transverse | ||||||
Temperatura de flexión bajo carga | 225 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 225 °C | dry | ISO 75-1/-2 | 2 MPa | |||||
245 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 245 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||||||
Temperatura de fusión | 255 °C Show Supplier Material materials with Temperatura de fusión of 255 °C | dry | ISO 11357-1/-3 | 10°C/min | |||||
Temperatura de reblandecimiento Vicat | 195 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 195 °C | ISO 306 | 50°C/h 50N | ||||||
Inflamabilidad | At thickness 1.6 mm IEC 60695-11-10: HB, At thickness 3.2 mm IEC 60695-11-10: HB |
Eléctrico
Property | Value | Condition | Frequency | Testing Standard | Comment |
---|---|---|---|---|---|
Constante dieléctrica | 3 [-] Show Supplier Material materials with Constante dieléctrica of 3 [-] | cond. | 100Hz | IEC 60250 | |
4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | IEC 60250 | 1MHz | |||
Factor de disipación | 0.016 [-] Show Supplier Material materials with Factor de disipación of 0.016 [-] | cond. | 1MHz | IEC 60250 | |
0.029 [-] Show Supplier Material materials with Factor de disipación of 0.029 [-] | cond. | 100Hz | IEC 60250 | ||
Rigidez dieléctrica | 34 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 34 kV/mm | cond., dry | IEC 60243-1 | ||
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | cond. | IEC 60093 | min. | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | cond. | IEC 60093 | min. | |
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | cond. | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.3 % Show Supplier Material materials with Contracción of 0.3 % | dry | ISO 294-4 | |
0.7 % Show Supplier Material materials with Contracción of 0.7 % | dry | ISO 294-4 | Transverse | |
Velocidad de flujo del volumen derretido | 7 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 7 cm³/10min | dry | ISO 1133 | 275°C/2.16kg |
Technological properties
Property | ||
---|---|---|
Application areas | Fittings, Components, and Injection Molded Parts | |
Fillers | 30% Glass Fiber | |
Processing methods | Injection Molding: |