General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 2.67 g/cm³ Show Supplier Material materials with Densidad of 2.67 g/cm³ |
Rugosidad superficial | 0.4 μm Show Supplier Material materials with Rugosidad superficial of 0.4 μm |
Medidas
Property | Value |
---|---|
Espesor | 6 - 610 mm Show Supplier Material materials with Espesor of 6 - 610 mm |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell (HBW) | 23.0 °C | 52 [-] Show Supplier Material materials with Dureza Brinell (HBW) of 52 [-] |
Elongación A50 | 23.0 °C | 16 % Show Supplier Material materials with Elongación A50 of 16 % |
Límite elástico | 23.0 °C | 80 MPa Show Supplier Material materials with Límite elástico of 80 MPa |
Módulo elástico | 23.0 °C | 70 GPa Show Supplier Material materials with Módulo elástico of 70 GPa |
Resistencia a la tracción | 23.0 °C | 190 MPa Show Supplier Material materials with Resistencia a la tracción of 190 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 900 J/(kg·K) Show Supplier Material materials with Calor específico of 900 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 2.39E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.39E-5 1/K | Mean values between 20°C and the mentioned temperature |
Conductividad térmica | 23.0 °C | 130 - 160 W/(m·K) Show Supplier Material materials with Conductividad térmica of 130 - 160 W/(m·K) |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 23.0 °C | 2.00E+7 - 2.30E+7 S/m Show Supplier Material materials with Conductividad eléctrica of 2.00E+7 - 2.30E+7 S/m |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminio | Balance | ||
Cobre | 0.1 % Show Supplier Material materials with Cobre of 0.1 % | ||
Cromo | 0.3 % Show Supplier Material materials with Cromo of 0.3 % | ||
Hierro | 0.4 % Show Supplier Material materials with Hierro of 0.4 % | ||
Magnesio | 2.6 - 3.6 % Show Supplier Material materials with Magnesio of 2.6 - 3.6 % | ||
Manganeso | 0.5 % Show Supplier Material materials with Manganeso of 0.5 % | ||
Otro | 0.15 % Show Supplier Material materials with Otro of 0.15 % | Total | |
Silicona | 0.4 % Show Supplier Material materials with Silicona of 0.4 % | ||
Titanio | 0.15 % Show Supplier Material materials with Titanio of 0.15 % | ||
Zinc | 0.2 % Show Supplier Material materials with Zinc of 0.2 % |
Technological properties
Property | ||
---|---|---|
Anodizing | very good | |
Application areas | Electronics and laser industry; Packaging technology; Optical industry; Medical technology; Display, semiconductor and solar systems | |
Corrosion properties | very good | |
Dimensional stability | very good | |
General machinability | very good | |
Processing methods | Homogenised and stress relieved: very good | |
Soldering general | bad | |
Welding | WIG: very good, MIG: very good |