Mecánica
Property | Value | Comment |
---|---|---|
Dureza Brinell | 265 - 310 [-] Show Supplier Material materials with Dureza Brinell of 265 - 310 [-] | as-delivered condition |
Dureza Rockwell C | 32 - 49 [-] Show Supplier Material materials with Dureza Rockwell C of 32 - 49 [-] | |
Resistencia a la tracción | 900 - 1060 MPa Show Supplier Material materials with Resistencia a la tracción of 900 - 1060 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 100 °C | 1.05e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.05e-05 1/K | for 20°C to the mentioned temperature |
150 °C | 1.07e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.07e-05 1/K | for 20°C to the mentioned temperature | |
200 °C | 1.08e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | for 20°C to the mentioned temperature | |
250 °C | 1.09e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.09e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.11e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.11e-05 1/K | for 20°C to the mentioned temperature | |
350 °C | 1.13e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.13e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.15e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.15e-05 1/K | for 20°C to the mentioned temperature | |
450 °C | 1.16e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.16e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.17e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.17e-05 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 23 °C | 23.5 W/(m·K) Show Supplier Material materials with Conductividad térmica of 23.5 W/(m·K) | |
150 °C | 24.2 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.2 W/(m·K) | ||
300 °C | 24.3 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.3 W/(m·K) | ||
350 °C | 24.4 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.4 W/(m·K) | ||
400 °C | 24.1 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.1 W/(m·K) | ||
500 °C | 23.2 W/(m·K) Show Supplier Material materials with Conductividad térmica of 23.2 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbono | 0.36 % Show Supplier Material materials with Carbono of 0.36 % |
Cromo | 16 % Show Supplier Material materials with Cromo of 16 % |
Hierro | Balance |
Manganeso | 0.9 % Show Supplier Material materials with Manganeso of 0.9 % |
Molibdeno | 1.2 % Show Supplier Material materials with Molibdeno of 1.2 % |
Silicona | 0.4 % Show Supplier Material materials with Silicona of 0.4 % |
Technological properties
Property | ||
---|---|---|
Application areas | As Formadur 2316 with highest demands on polishability | |
Heat Treatment | Soft annealing: 760-800°C (Cooling in furnace) - Hardening: 1020-1050°C and quenching in oil or salt bath 500-520°C |