Medidas
Property | Value |
---|---|
Diámetro | 21 - 755 mm Show Supplier Material materials with Diámetro of 21 - 755 mm |
Mecánica
Property | Value | Comment |
---|---|---|
Dureza Brinell | 355 - 410 [-] Show Supplier Material materials with Dureza Brinell of 355 - 410 [-] | as-delivered condition |
Dureza Rockwell C | 56 - 58 [-] Show Supplier Material materials with Dureza Rockwell C of 56 - 58 [-] | after quenching |
Resistencia a la tracción | 1190 - 1385 MPa Show Supplier Material materials with Resistencia a la tracción of 1190 - 1385 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 100 °C | 1.22e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.22e-05 1/K | for 20°C to the mentioned temperature |
200 °C | 1.3e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.33e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.33e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.37e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.37e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.42e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.42e-05 1/K | for 20°C to the mentioned temperature | |
600 °C | 1.44e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.44e-05 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 23 °C | 36 W/(m·K) Show Supplier Material materials with Conductividad térmica of 36 W/(m·K) | |
350 °C | 38.8 W/(m·K) Show Supplier Material materials with Conductividad térmica of 38.8 W/(m·K) | ||
700 °C | 35 W/(m·K) Show Supplier Material materials with Conductividad térmica of 35 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbono | 0.56 % Show Supplier Material materials with Carbono of 0.56 % |
Cromo | 1.1 % Show Supplier Material materials with Cromo of 1.1 % |
Hierro | Balance |
Manganeso | 0.75 % Show Supplier Material materials with Manganeso of 0.75 % |
Níquel | 1.7 % Show Supplier Material materials with Níquel of 1.7 % |
Silicona | 0.25 % Show Supplier Material materials with Silicona of 0.25 % |
Vanadio | 0.1 % Show Supplier Material materials with Vanadio of 0.1 % |
Technological properties
Property | ||
---|---|---|
Application areas | Standard steel for forging dies, press dies, auxiliary tools for extrusion, die holders, armoured trim dies, hot shear blades | |
Heat Treatment | Soft annealing: 650-700°C (Cooling in furnace) - Hardening: 830-870°C, 860-900 (Oil, Air) |