Medidas
Property | Value |
---|---|
Ancho | 1010 mm Show Supplier Material materials with Ancho of 1010 mm |
Espesor | 30 - 80 mm Show Supplier Material materials with Espesor of 30 - 80 mm |
Mecánica
Property | Value | Comment |
---|---|---|
Dureza Brinell | 250 [-] Show Supplier Material materials with Dureza Brinell of 250 [-] | soft annealed |
Dureza Rockwell C | 58 - 62 [-] Show Supplier Material materials with Dureza Rockwell C of 58 - 62 [-] |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 100 °C | 1.09e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.09e-05 1/K | for 20°C to the mentioned temperature |
200 °C | 1.19e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.23e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.23e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.26e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.26e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.29e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.29e-05 1/K | for 20°C to the mentioned temperature | |
600 °C | 1.3e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | for 20°C to the mentioned temperature | |
700 °C | 1.32e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.32e-05 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 20 °C | 16.7 W/(m·K) Show Supplier Material materials with Conductividad térmica of 16.7 W/(m·K) | |
350 °C | 20.5 W/(m·K) Show Supplier Material materials with Conductividad térmica of 20.5 W/(m·K) | ||
700 °C | 24.2 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.2 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbono | 2.1 % Show Supplier Material materials with Carbono of 2.1 % |
Cromo | 12 % Show Supplier Material materials with Cromo of 12 % |
Hierro | Balance |
Manganeso | 0.35 % Show Supplier Material materials with Manganeso of 0.35 % |
Silicona | 0.35 % Show Supplier Material materials with Silicona of 0.35 % |
Wolframio | 0.7 % Show Supplier Material materials with Wolframio of 0.7 % |
Technological properties
Property | ||
---|---|---|
Application areas | Blanking dies for cutting transformer and dynamo sheets, paper and plastics, deep-drawing tools, drawing dies and mandrels, shear blades | |
Heat Treatment | Soft annealing: 800-840°C (Cooling in furnace) - Stress-relief-annealing: 650-700°C (cooling in Furnace), Hardening: 950-980°C and quenching in oil, air or salt bath: 500-550°C |