Tempered mould steel with improved quenching and tempering properties, good machinability, polishable, weldable and can be textured. This grade offers substantial improvements, especially for building larger and complex moulds. Specific modifications of the grade's components as well as additional smelting and secondary metallurgy ensure Formadur® 320's outstanding properties. We recommend the use of Formadur® 320 Superclean (ESR) for the highest demands.

Los datos sobre este material han sido proporcionados por Deutsche Edelstahlwerke Specialty Steel (DEW).

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

Propiedades

Mecánica

PropertyValueComment

Dureza Brinell

280 - 385 [-]

Show Supplier Material materials with Dureza Brinell of 280 - 385 [-]

as-delivered condition

Dureza Rockwell C

28 - 51 [-]

Show Supplier Material materials with Dureza Rockwell C of 28 - 51 [-]

Resistencia a la tracción

1060 - 1190 MPa

Show Supplier Material materials with Resistencia a la tracción of 1060 - 1190 MPa

Aplicaciones térmicas

PropertyTemperatureValueComment

Coeficiente de dilatación térmica

100 °C

1.11e-05 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 1.11e-05 1/K

for 20°C to the mentioned temperature

200 °C

1.29e-05 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 1.29e-05 1/K

for 20°C to the mentioned temperature

300 °C

1.34e-05 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 1.34e-05 1/K

for 20°C to the mentioned temperature

400 °C

1.35e-05 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 1.35e-05 1/K

for 20°C to the mentioned temperature

500 °C

1.38e-05 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 1.38e-05 1/K

for 20°C to the mentioned temperature

600 °C

1.41e-05 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K

for 20°C to the mentioned temperature

700 °C

1.43e-05 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 1.43e-05 1/K

for 20°C to the mentioned temperature

Conductividad térmica

23 °C

36 W/(m·K)

Show Supplier Material materials with Conductividad térmica of 36 W/(m·K)

150 °C

37.4 W/(m·K)

Show Supplier Material materials with Conductividad térmica of 37.4 W/(m·K)

300 °C

33 W/(m·K)

Show Supplier Material materials with Conductividad térmica of 33 W/(m·K)

Chemical properties

PropertyValue

Carbono

0.34 %

Show Supplier Material materials with Carbono of 0.34 %

Cromo

1.7 %

Show Supplier Material materials with Cromo of 1.7 %

Hierro

Balance

Manganeso

0.8 %

Show Supplier Material materials with Manganeso of 0.8 %

Molibdeno

0.4 %

Show Supplier Material materials with Molibdeno of 0.4 %

Níquel

0.5 %

Show Supplier Material materials with Níquel of 0.5 %

Silicona

0.4 %

Show Supplier Material materials with Silicona of 0.4 %

Technological properties

Property
Application areas

As Formadur 320 with highest demands on polishability

Heat Treatment

Soft annealing: 710-740°C (Cooling in furnace) - Hardening: 820-850°C and quenching in oil or polymer