General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 20.59 g/cm³ Show Supplier Material materials with Densidad of 20.59 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Vickers | 23.0 °C | 82 [-] Show Supplier Material materials with Dureza Vickers of 82 [-] |
Elongación | 20.0 °C | 39 % Show Supplier Material materials with Elongación of 39 % |
1200.0 °C | 59 % Show Supplier Material materials with Elongación of 59 % | |
1400.0 °C | 68 % Show Supplier Material materials with Elongación of 68 % | |
1600.0 °C | 71 % Show Supplier Material materials with Elongación of 71 % | |
Límite elástico Rp 0,2 | 20.0 °C | 128 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 128 MPa |
1200.0 °C | 40 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 40 MPa | |
1400.0 °C | 27 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 27 MPa | |
1600.0 °C | 16.1 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 16.1 MPa | |
Módulo elástico | 23.0 °C | 106 GPa Show Supplier Material materials with Módulo elástico of 106 GPa |
Resistencia a la tracción | 20.0 °C | 290 MPa Show Supplier Material materials with Resistencia a la tracción of 290 MPa |
1200.0 °C | 55.3 MPa Show Supplier Material materials with Resistencia a la tracción of 55.3 MPa | |
1400.0 °C | 31.2 MPa Show Supplier Material materials with Resistencia a la tracción of 31.2 MPa | |
1600.0 °C | 19.2 MPa Show Supplier Material materials with Resistencia a la tracción of 19.2 MPa | |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Conductividad térmica | 20.0 °C | 45.2 W/(m·K) Show Supplier Material materials with Conductividad térmica of 45.2 W/(m·K) |
1200.0 °C | 72.6 W/(m·K) Show Supplier Material materials with Conductividad térmica of 72.6 W/(m·K) | |
1400.0 °C | 74.7 W/(m·K) Show Supplier Material materials with Conductividad térmica of 74.7 W/(m·K) | |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.7E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.7E-7 Ω·m |
1146.0 °C | 5.3E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 5.3E-7 Ω·m | |
1369.0 °C | 6E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 6E-7 Ω·m | |